A coal tar pitch modification technology, applied in building components, building insulation materials, construction, etc., can solve the problems of single modifier and mixed use that have not received widespread attention, so as to achieve convenient processing, increase use value, and alleviate supply shortage Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] Weigh the following raw materials in parts by weight:
[0018] 90 parts of coal tar pitch
[0019] 4 parts p-tolualdehyde
[0020] Polycarbonate 2.1 parts
[0021] Coumarone-indene resin 2.7 parts
[0022] Bisphenol A type unsaturated polyester resin 1.9 parts
[0023] 5 parts of polyphosphoric acid;
[0024] Add p-tolualdehyde, polycarbonate, bisphenol A unsaturated polyester resin, coumarone-indene resin and polyphosphoric acid to the base coal tar pitch, mix and melt at 170-200°C and then pass through a colloid mill Grinding and shearing for 30-40 minutes to uniformly disperse in the asphalt cement to obtain the modified coal tar pitch of the present invention.
Embodiment 2
[0026] Weigh the following raw materials in parts by weight:
[0027] 90 parts of coal tar pitch
[0028] 2 parts p-methylbenzaldehyde
[0029] Polycarbonate 1.2 parts
[0030] Coumarone-indene resin 2.3 parts
[0031] Bisphenol A type unsaturated polyester resin 1.5 parts
[0032] 4 parts polyphosphoric acid.
[0033] Add p-tolualdehyde, polycarbonate, bisphenol A unsaturated polyester resin, coumarone-indene resin and polyphosphoric acid to the base coal tar pitch, mix and melt at 170-200°C and then pass through a colloid mill Grinding and shearing for 30-40 minutes to uniformly disperse in the asphalt cement to obtain the modified coal tar pitch of the present invention.
Embodiment 3
[0035] Weigh the following raw materials in parts by weight:
[0036] 90 parts of coal tar pitch
[0037] 2 parts p-methylbenzaldehyde
[0038] Polycarbonate 2.1 parts
[0039] Coumarone-indene resin 2.7 parts
[0040] Bisphenol A type unsaturated polyester resin 1.5 parts
[0041] 5 parts of polyphosphoric acid.
[0042] Add p-tolualdehyde, polycarbonate, bisphenol A unsaturated polyester resin, coumarone-indene resin and polyphosphoric acid to the base coal tar pitch, mix and melt at 170-200°C and then pass through a colloid mill Grinding and shearing for 30-40 minutes to uniformly disperse in the asphalt cement to obtain the modified coal tar pitch of the present invention.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com