Carried-type active platinum metal bunch, prepn. method and use thereof
A platinum metal and supported technology, which is applied in the field of supported active platinum metal clusters and its preparation, can solve the problems of narrow anti-tumor spectrum, duration of adverse reactions, toxic and side effects, etc., and achieves simple implementation method, solution stability and The effect of spreading the problem
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] Preparation: According to "Oral vanadium supplementation agent with bimetallic oxide as carrier and its preparation and application method" Ye Ying, Feng Lujia, Zheng Libo, Shen Zhongyue, Han Jie, Chen Zhifei, Li Shanshan. National invention patent authorization announcement number CN 1187091C) method to prepare hydrotalcite.
[0025] 1) Grind the hydrotalcite obtained in the preparatory step to 400 mesh, add water and stir evenly, and make a suspension slurry with a concentration of 10%:
[0026] 2) chloroplatinic acid hexahydrate (H 2 PtCl 6 ·6H 2 O), pre-mixed into 0.5g / L aqueous solution;
[0027] 3) Slowly add the chloroplatinic acid solution in step 2) into the suspension slurry in step 1), then add vitamin C whose molar ratio is 3-times that of chloroplatinic acid, and react at room temperature for 4 hours under a nitrogen atmosphere;
[0028]4) centrifuging the reaction solution obtained in step 3) under a nitrogen atmosphere, washing with water, and centrif...
Embodiment 2
[0031] Preparation: Prepare water according to the method of "A Method for Preparing Double Metal Oxide and Hydrotalcite" (Ye Ying, Li Shanshan, Chen Zhifei, Zheng Libo, Huang Xia, Wu Daidai, Han Jie, Zhang Weirui. National Invention Patent Grant No. CN 1222467C) talc.
[0032] 1) Grind the hydrotalcite obtained in the preparatory step to 500 mesh, add water and stir evenly, and make a suspension slurry with a concentration of 5%:
[0033] 2) chloroplatinic acid with a platinum content of 10% by weight of hydrotalcite is prepared in advance into a 25g / L aqueous solution;
[0034] 3) Slowly add the chloroplatinic acid solution in step 2) into the suspension slurry in step 1), then add sodium borohydride whose molar ratio is 10 times that of chloroplatinic acid, and react at room temperature for 10 hours under a nitrogen atmosphere;
[0035] 4) The reaction solution obtained in step 3) is filtered and separated under an argon atmosphere, washed with water and dehydrated by filt...
Embodiment 3
[0038] 1) Calcining commercially available hydrotalcite at 450°C to obtain a bimetallic oxide, then grinding to 500 mesh, adding water and stirring evenly, to prepare a suspension slurry with a concentration of 1%:
[0039] 2) chloroplatinic acid with a platinum content of 20% by weight of the double metal oxide is prepared in advance into a 50 g / L aqueous solution;
[0040] 3) Slowly add the chloroplatinic acid solution in step 2) into the suspension slurry in step 1), then add potassium borohydride whose molar ratio is 15 times that of chloroplatinic acid, and react at room temperature under an argon atmosphere for 15 hours;
[0041] 4) The reaction solution obtained in step 3) is filtered and separated under an argon atmosphere, washed with water, and centrifuged for dehydration;
[0042] 5) The filter cake obtained in step 4) is vacuum-dried at a temperature lower than 80° C. and crushed to 400 meshes to obtain supported active platinum metal clusters. The content of plati...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com