Embodiment 1
[0030] The process formula of the present invention is: water 1000kg; polyvinyl alcohol 0588 is 100kg; polyvinylpyrrolidone 25kg; boric acid 3kg; acrylamide 50kg; ammonium persulfate 0.06kg; sodium bisulfite 0.06kg; Sodium alkylbenzene sulfonate 3.3kg; Sorbitan monostearate 3.3kg; Alkylphenol polyoxyethylene ether 3.3kg.
[0031] Its process operation steps are as follows:
[0032] Step 1: Dissolution and Crosslinking
[0033] Add 890kg of water, 100kg of polyvinyl alcohol 0588, 25kg of polyvinylpyrrolidone, and 3kg of boric acid into a 1.5-ton reactor with a stirrer, heat up and dissolve, and keep warm at 80°-85°C for 1.5 hours until completely dissolved. , boric acid has completed the cross-linking reaction with polyvinyl alcohol, but has no effect on dissolution.
[0034] Step 2: Polymerization
[0035] When the temperature is lowered to 52°-54°C, add 50kg of acrylamide and 100kg of water to make a liquid at one time, mix for 10-30 minutes, then add the ammonium persulfa...
Embodiment 2
[0041] The process formula of the present invention is: water 1000kg; polyvinyl alcohol 0588 is 120kg; polyvinylpyrrolidone 25kg; boric acid 3.5kg; acrylamide 35kg; ammonium persulfate 0.08kg; sodium bisulfite 0.08kg; Sodium dialkylbenzene sulfonate 3.2kg; Sorbitan monostearate 3.2kg; Alkylphenol polyoxyethylene ether 3.2kg.
[0042] Its process operation steps are as follows:
[0043] Step 1: Dissolution and Crosslinking
[0044] Add 890kg of water, 120kg of polyvinyl alcohol 0588, 25kg of polyvinylpyrrolidone, and 3.5kg of boric acid into a 1.5-ton reactor with a stirrer, heat up and dissolve, and keep warm at 80°-85°C for 1.5 hours until completely dissolved. At the same time, boric acid has completed the cross-linking reaction with polyvinyl alcohol, but has no effect on dissolution.
[0045] Step 2: Polymerization
[0046] When the temperature is lowered to 52°-54°C, add 35kg of acrylamide and 100kg of water into a liquid at one time, dissolve for 10-30 minutes, then a...
Embodiment 3
[0052] The process formula of the present invention is: water 1000kg; polyvinyl alcohol 0588 is 150kg; polyvinylpyrrolidone 20kg; boric acid 4.5kg; acrylamide 30kg; ammonium persulfate 0.1kg; sodium bisulfite 0.1kg; Sodium dialkylbenzene sulfonate 2kg; sorbitan monostearate 2kg; alkylphenol polyoxyethylene ether 2kg.
[0053] Its process operation steps are as follows:
[0054] Step 1: Dissolution and Crosslinking
[0055]Add 890kg of water, 150kg of polyvinyl alcohol 0588, 20kg of polyvinylpyrrolidone, and 4.5kg of boric acid into a 1.5-ton reactor with a stirrer, heat up and dissolve, and keep warm at 80°-85°C for 1.5 hours until completely dissolved. At the same time, boric acid has completed the cross-linking reaction with polyvinyl alcohol, but has no effect on dissolution.
[0056] Step 2: Polymerization
[0057] When the temperature is lowered to 52°-54°C, add 30kg of acrylamide and 100kg of water into a liquid at one time, dissolve for 10-30 minutes, then add the am...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com