An inorganic nano- and nano-silica technology, applied in the field of waterproof liquid preparation, can solve the problems of impermeability, resistance to chloride ion erosion, rapid setting of silicate, etc., and achieve superior hydrophobic performance and super self-healing ability. , Good alkali resistance effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0022] Sodium silicate: 20 parts, 30 parts of nano-silica emulsion, 2 parts of lithium magnesium silicate, 8 parts of silane coupling agent, 0.02 part of surfactant, 5 parts of mica powder, 0.3 part of regulator, 0.3 part of coagulation accelerator , 0.5 part of metal ion chelating agent, 0.2 part of antifreeze, 100 parts of deionized water.
[0023] Specifically, the preparation steps of the waterproof liquid are:
[0024] (1) Put 20 parts of deionized water into the high-speed mixer, add 5 parts of mica powder, 0.3 parts of regulator, 0.3 parts of coagulant, 0.5 parts of metal ion chelating agent, 0.2 parts of antifreeze, mix and stir evenly to form a mixed solution a.
[0025] (2) Add 80 parts of deionized water to the reaction kettle, then add 30 parts of nano-silica emulsion, heat to 50-60°C, add 0.02 parts of surfactant, 8 parts of silane coupling agent, and 20 parts of silicic acid in sequence Sodium, 2 parts of magnesium lithium silicate until completely dissolved, c...
Embodiment 2
[0028] Sodium silicate: 20 parts, 20 parts of nano-silica emulsion, 1 part of lithium magnesium silicate, 8 parts of silane coupling agent, 0.02 part of surfactant, 5 parts of mica powder, 0.3 part of regulator, 0.3 part of coagulation accelerator , 0.5 part of metal ion chelating agent, 0.2 part of antifreeze, 100 parts of deionized water.
[0029] Specifically, the preparation steps of the waterproof liquid are:
[0030] (1) Add 20 parts of deionized water into the high-speed mixer, and sequentially add 5 parts of mica powder, 0.3 parts of regulator, 0.3 parts of coagulant, 0.5 parts of metal ion chelating agent, 0.2 parts of antifreeze, mix and stir evenly to form Mixture a;
[0031] (2) Then add 80 parts of deionized water to the reactor, add 20 parts of nano-silica emulsion, heat to 50-60°C, add 0.02 parts of surfactant, 8 parts of silane coupling agent, and 20 parts of sodium silicate in sequence 1 part of lithium magnesium silicate until completely dissolved, cooled a...
Embodiment 3
[0034] Sodium silicate: 30 parts, 20 parts of nano-silica emulsion, 2 parts of lithium magnesium silicate, 10 parts of silane coupling agent, 0.2 part of surfactant, 5 parts of mica powder, 0.3 part of regulator, 0.3 part of coagulation accelerator , 5 parts of metal ion chelating agent, 2 parts of antifreeze, 100 parts of deionized water.
[0035] Specifically, the preparation steps of the waterproof liquid are:
[0036] (1) Put 20 parts of deionized water into the high-speed mixer, add 5 parts of mica powder, 0.3 parts of regulator, 0.3 parts of coagulation accelerator, 5 parts of metal ion chelating agent, and 2 parts of antifreeze in turn, mix and stir evenly to form a mixed liquid a.
[0037] (2) Add 80 parts of deionized water to the reaction kettle, add 20 parts of nano-silica emulsion, heat to 50-60°C, add 0.2 parts of surfactant, 10 parts of silane coupling agent, and 30 parts of sodium silicate in sequence 2 parts of lithium magnesium silicate were completely disso...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com