A technology of oxide electrical and contact materials, which is applied in the direction of contacts, circuits, and electrical switches, and can solve the problems of improving the anti-welding performance of unsuitable materials, reducing the electrical conductivity of electrical contact materials, and not improving the anti-welding performance. , to achieve the effect of improving the anti-welding performance, reducing the welding force and reducing the tensile strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0031] a) 17.6kg silver plates are melted in a graphite crucible to form a silver melt;
[0032] b) The temperature of the silver melt is increased to 1300°C, and 0.2kg of nickel powder is added;
[0033] c) sufficient stirring to form a homogenized alloy melt;
[0034] d) The temperature of the silver alloy melt is lowered to 1050°C, 2.2kg of cadmium ingots and additives are added, and the alloy is fully stirred to form an alloy;
[0035] e) AgCd10.5 alloy is cast into a round ingot, and the mass percentage of nickel element in the alloy ingot is 1%;
[0036] f) After extrusion, hot rolling, cold rolling, punching, internal oxidation and other processes, it is processed into internal oxidation AgCdO (12) sheet contacts.
Embodiment 2
[0038] a) 17.28kg silver plates are melted in a graphite crucible to form a silver melt;
[0039] b) The temperature of the silver melt is increased to 1250°C, and 0.8kg of AgNi10 alloy is added;
[0040] c) sufficient stirring to form a homogenized alloy melt;
[0041] d) The temperature of the silver alloy melt is lowered to 1100° C., adding 1.26 kg of tin ingot and 0.66 kg of indium ingot, and fully stirring to form an alloy;
[0042]e) AgSn6.3In3.3 alloy is cast into a round ingot, and the mass percentage of nickel element in the alloy ingot is 0.4%;
[0043] f) After extrusion, drawing, internal oxidation, secondary extrusion and other processes, it is processed into internal oxidation AgSnO 2 (8)In 2 o 3 (4) wire.
Embodiment 3
[0045] a) 18.26kg silver plates are melted in a graphite crucible to form a silver melt;
[0046] b) The temperature of the silver melt is increased to 1300°C, and 0.14kg of nickel powder is added;
[0047] c) sufficient stirring to form a homogenized alloy melt;
[0048] d) The temperature of the silver alloy melt is lowered to 1050° C., adding 1.6 kg of zinc ingot, and fully stirring to form an alloy;
[0049] e) AgZn8 alloy is cast into a round ingot, and the mass percentage of nickel element in the alloy ingot is 0.7%;
[0050] f) After extrusion, hot rolling, cold rolling, punching, internal oxidation and other processes, it is processed into internal oxidation AgZnO (10) sheet contacts.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com