Gold nanorod-lipid polymer vesicle with transdermal delivery function and preparation method and application of gold nanorod-lipid polymer vescle
A technology of gold nanorods and nanovesicles, which is applied in the field of medicine, can solve the problems of destroying the structure of the stratum corneum of the skin and skin irritation, and achieve the effects of enhancing transdermal efficiency, promoting release, and good biocompatibility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0038] Preparation of gold nanorod-lipopolymer vesicles
[0039] (1) Preparation of polymer PSAA
[0040]Using a high-pressure reactor as a reactor, allyl alcohol (AA), dicumyl peroxide (DCP) and styrene (ST) are added to the reactor, nitrogen is used as a protective agent, and allyl alcohol and styrene are used as The mass of the two reaction raw materials is 0.5g and 0.5g respectively, dicumyl peroxide is used as the initiator, the addition amount is 1mg, the reaction temperature is 50°C, and the reaction time is 1h, and the polymer PSAA is finally obtained.
[0041] (2) Preparation of lipopolymer vesicles
[0042] Under pulsed ultrasound, the polymer 5gPSAA was mixed with 5mL ultrapure water, and dioleoylphosphatidylethanolamine and (2,3-dioleoyl-propyl)-trimethylamine mixed in any ratio were added as surfactants. The quality of the surfactant is 1 mg, and lipopolymer vesicles are prepared.
[0043] (3) Preparation of gold nanorods
[0044] When light is incident on the...
Embodiment 2
[0051] Preparation of gold nanorod-lipopolymer vesicles
[0052] (1) Preparation of polymer PSAA
[0053] Using a high-pressure reactor as a reactor, allyl alcohol (AA), dicumyl peroxide (DCP) and styrene (ST) are added to the reactor, nitrogen is used as a protective agent, and allyl alcohol and styrene are used as The mass of the two reaction raw materials is 5g and 0.5g respectively, dicumyl peroxide is used as the initiator, the addition amount is 550mg, the reaction temperature is 150°C, and the reaction time is 10h, and the polymer PSAA is finally obtained.
[0054] (2) Preparation of lipopolymer vesicles
[0055] Under pulsed ultrasound, the polymer 5gPSAA was mixed with 50mL ultrapure water, and dioleoylphosphatidylethanolamine and (2,3-dioleoyl-propyl)-trimethylamine mixed in any ratio were added as surfactants. The quality of the surfactant was 550mg, and the lipopolymer vesicles were prepared.
[0056] (3) Preparation of gold nanorods
[0057] When light is inci...
Embodiment 3
[0064] Validation of gold nanorod-lipopolymer vesicles
[0065] (1) Particle size measurement of gold nanorod-lipopolymer vesicles
[0066] First use ultrapure water to adjust the gold nanorods synthesized in Example 1 to 100 μg / mL, and measure the size of the gold nanorods under the Malvern laser particle size analyzer, the results are as follows figure 1 shown.
[0067] Use ultrapure water to adjust the lipopolymer vesicles synthesized in Example 1 to 100 μg / mL, measure the size of lipopolymer vesicles under the Malvern laser particle size analyzer, the results are as follows figure 2 shown.
[0068] Use ultrapure water to adjust the gold nanorods-lipopolymer vesicles synthesized in Example 1 to 100 μg / mL, and measure the size of the gold nanorods-lipopolymer vesicles under the Malvern laser particle sizer, the result Such as image 3 shown.
[0069] (2) Morphological observation of gold nanorods
[0070] Get the gold nanorod solution of Example 1, drop it on a dedica...
PUM
Property | Measurement | Unit |
---|---|---|
Particle size | aaaaa | aaaaa |
Particle size | aaaaa | aaaaa |
Molecular weight | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com