A kind of high penetration bonded magnet and preparation method thereof
A technology of bonded magnets and magnetic powders, applied in the field of magnetic therapy, can solve the problems of low operating temperature, low magnetic storage capacity and high demagnetization rate, and achieve the effects of extending service life, excellent mechanical properties and good corrosion resistance.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0069] A high-penetration bonded magnet, the mass ratio of the components of the bonded magnet is as follows: 48 parts of magnetic powder, 4 parts of chlorinated polyethylene and 0.4 part of epoxy soybean oil.
[0070] A preparation method of a high penetration bonded magnet, comprising the following steps:
[0071] (1) Take each component according to the ratio of parts by mass, and grind a quarter of the magnetic powder at 30°C for 1 hour to obtain component A;
[0072] Add component A, remaining magnetic powder, epoxidized soybean oil and chlorinated polyethylene into the mixer and mix thoroughly for 8 minutes, then take out mixture 2;
[0073] (2) Use an internal mixer for internal mixing, the pressure is 0.8Mpa, the rotor speed is 75r / min, and the temperature is set at 110°C. Put the mixture 2 into the internal mixing chamber first, and after internal mixing for 3 minutes, raise the temperature to 135°C for internal mixing 5 minutes, then lower the temperature to 120°C, ...
Embodiment 2
[0079] A high-penetration bonded magnet. The mass ratio of the components of the bonded magnet is as follows: 64 parts of magnetic powder, 4 parts of chlorinated polyethylene, and 0.4 part of epoxy soybean oil.
[0080] A preparation method of a high penetration bonded magnet, comprising the following steps:
[0081] (1) Take each component according to the ratio of parts by mass, and grind a quarter of the magnetic powder at 30°C for 1 hour to obtain component A;
[0082] Add component A, remaining magnetic powder, epoxidized soybean oil and chlorinated polyethylene into the mixer and mix thoroughly for 8 minutes, then take out mixture 2;
[0083] (2) Use an internal mixer for internal mixing, the pressure is 0.8Mpa, the rotor speed is 75r / min, and the temperature is set at 110°C. Put the mixture 2 into the internal mixing chamber first, and after internal mixing for 3 minutes, raise the temperature to 135°C for internal mixing 5 minutes, then lower the temperature to 120°C,...
Embodiment 3
[0089] A high-penetration bonded magnet, the mass ratio of the components of the bonded magnet is as follows: 80 parts of magnetic powder, 4 parts of chlorinated polyethylene and 0.4 part of epoxy soybean oil.
[0090] A preparation method of a high penetration bonded magnet, comprising the following steps:
[0091] (1) Take each component according to the ratio of parts by mass, and grind a quarter of the magnetic powder at 30°C for 1 hour to obtain component A;
[0092] Add component A, remaining magnetic powder, epoxidized soybean oil and chlorinated polyethylene into the mixer and mix thoroughly for 8 minutes, then take out mixture 2;
[0093] (2) Use an internal mixer for internal mixing, the pressure is 0.8Mpa, the rotor speed is 75r / min, and the temperature is set at 110°C. Put the mixture 2 into the internal mixing chamber first, and after internal mixing for 3 minutes, raise the temperature to 135°C for internal mixing 5 minutes, then lower the temperature to 120°C, ...
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
width | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com