Preserve silk cotton fabric and preparation method thereof
A fabric and silk cotton technology, applied in the field of anti-corrosion silk cotton fabric and its preparation, can solve the problems of skin irritation, wrinkling, and insufficient elasticity, so as to increase gloss and softness, balance oil secretion, enhance The effect of water resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] In the embodiment of the present invention, a kind of anti-corrosion silk cotton fabric, the raw material according to weight part comprises: 45 parts of Tencel cotton, 35 parts of poultry feathers, 0.5 part of silane coupling agent KH550, 12 parts of chitosan, 0.5 part of spun silk fiber , 0.5 parts of bamboo leaf powder, 0.5 parts of jojoba oil, 5 parts of starch, 0.5 parts of white oil, 2 parts of rosemary, 50 parts of ramie fiber, and 5 parts of water.
[0020] The preparation method of described anticorrosion silk cotton fabric, comprises the following specific steps:
[0021] (1) Add jojoba oil to water, add chitosan while stirring.
[0022] (2) Add starch, stir for 8 minutes, and spray dry to obtain modified starch.
[0023] (3) Grinding tencel cotton, poultry feathers, spun silk fibers, ramie fibers, and rosemary into 400-mesh fiber particles.
[0024] (4) The fiber particles and the silane coupling agent KH550 are mixed and stirred evenly, and then fed into a...
Embodiment 2
[0029] In the embodiment of the present invention, a kind of anti-corrosion silk cotton fabric, the raw material according to weight part comprises: Tencel cotton 60 parts, poultry feather 65 parts, silane coupling agent KH550 4 parts, chitosan 22 parts, spun silk fiber 5 parts , 4 parts of bamboo leaf powder, 4 parts of jojoba oil, 12 parts of starch, 4 parts of white oil, 8 parts of rosemary, 60 parts of ramie fiber, and 15 parts of water.
[0030] The preparation method of described anticorrosion silk cotton fabric, comprises the following specific steps:
[0031] (1) Add jojoba oil to water, add chitosan while stirring.
[0032] (2) Add starch, stir for 18 minutes, and spray dry to obtain modified starch.
[0033] (3) Crush Tencel cotton, poultry feathers, spun silk fibers, ramie fibers, and rosemary into 600-mesh fiber particles.
[0034] (4) The fiber particles and the silane coupling agent KH550 are mixed and stirred evenly, and then fed into a twin-screw extruder to ...
Embodiment 3
[0039] In the embodiment of the present invention, a kind of anti-corrosion silk cotton fabric, the raw material according to weight part comprises: Tencel cotton 48 parts, poultry feather 40 parts, silane coupling agent KH550 1 part, chitosan 14 parts, spun silk fiber 1 part , 1 part of bamboo leaf powder, 1 part of jojoba oil, 7 parts of starch, 1 part of white oil, 4 parts of rosemary, 54 parts of ramie fiber, and 8 parts of water.
[0040] The preparation method of described anticorrosion silk cotton fabric, comprises the following specific steps:
[0041] (1) Add jojoba oil to water, add chitosan while stirring.
[0042] (2) Add starch, stir for 10 minutes, and spray dry to obtain modified starch.
[0043] (3) Grinding tencel cotton, poultry feathers, spun silk fibers, ramie fibers, and rosemary into 450-mesh fiber particles.
[0044] (4) The fiber particles and the silane coupling agent KH550 are mixed and stirred evenly, and then fed into a twin-screw extruder to make...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com