A kind of calcification transition-leaching method for decomposing bastnaesite

A technology of calcification transformation and bastnaesite, which is applied in the field of calcification transformation-leaching and decomposition of bastnaesite, can solve the problems of rare earth loss, reduction of rare earth recovery rate, waste of fluorine resources, etc., achieve efficient separation and comprehensive recovery, and realize green Effect of cleaner production and reduction of fuel consumption

Active Publication Date: 2014-10-01
NORTHEASTERN UNIV LIAONING
View PDF9 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The above process has the advantages of short process flow, small investment, and low production cost of cerium products, but there are problems such as discontinuous process, low product purity, difficult recovery of thorium and fluorine dispersed in slag and waste water, and pollution to the environment.
For example, Chinese Patent (Application No.) 200410031180.6 discloses a method for decomposing bastnaesite with hydrochloric acid. In this method, after oxidizing and roasting bastnaesite, sodium hydroxide is used to remove fluoride, and hydrochloric acid is optimally soluble-completely soluble. In this method, hydrogen The consumption of sodium oxide is large, and a large amount of alkaline wastewater is produced at the same time
Chinese patents (application numbers) 2004100031179.3 and 200410070199.1 disclose a method for decomposing bastnaesite by sulfuric acid leaching. These methods all have defects such as high energy consumption, large amount of waste water and serious pollution, and serious waste of fluorine resources
The impurities in the concentrate will significantly affect the product quality and reduce the recovery rate of rare earths. Therefore, the concentrate must be removed by chemical beneficiation before decomposing impurity minerals such as fluorspar, but the rare earths will lose 2%-5% during the beneficiation process
The process of decomposing Baotou rare earth concentrate by sodium hydroxide method is relatively mature, but it is rarely used in domestic large-scale factories because of the disadvantages of high grade rare earth concentrate, impurity removal treatment before decomposition and low recovery rate of rare earth.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A kind of calcification transition-leaching method for decomposing bastnaesite

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0031] (1) Activation pretreatment of rare earth concentrate

[0032] Roast bastnaesite concentrate at 430°C for 3 hours to obtain activated ore;

[0033] (2) Activated ore calcification transition pretreatment

[0034] Mix the activated ore obtained in step (1) with CaO evenly at a mass ratio of 100:70, then mix the mixture with 0.5mol / L NaOH solution at a solid-to-liquid ratio of 1kg:20L for calcification and fluorine-fixing transition pretreatment, and the transition temperature is 150°C, the transformation time is 3 hours, and then solid-liquid separation is carried out to obtain transformation slag and lye, and the lye is directly recycled;

[0035] (3) Transformation slag acid leaching

[0036] (3a) The transformation slag obtained in step (2) and 1mol / L hydrochloric acid solution are subjected to acid leaching treatment according to the solid-to-liquid ratio of 1kg:20L, the leaching temperature is 30°C, the leaching time is 120min, and the mass fraction added during t...

Embodiment 2

[0042] (1) Activation pretreatment of rare earth concentrate

[0043] Roast bastnaesite concentrate at 480°C for 2 hours to obtain activated ore;

[0044] (2) Activated ore calcification transition pretreatment

[0045] Mix the activated ore obtained in step (1) with CaO evenly at a mass ratio of 100:80, then mix the mixture with 0.5mol / L NaOH solution at a solid-to-liquid ratio of 1kg:15L for calcification and fluorine-fixing transition pretreatment, and the transition temperature is 180°C, the transformation time is 2 hours, and then the solid-liquid separation is carried out to obtain the transformation slag and lye, and the lye is directly recycled;

[0046] (3) Transformation slag acid leaching

[0047] (3a) The transformation slag obtained in step (2) and 1.5mol / L hydrochloric acid solution were subjected to acid leaching treatment according to the solid-to-liquid ratio of 1kg:20L, the leaching temperature was 50°C, the leaching time was 90min, and the mass fraction ad...

Embodiment 3

[0053] (1) Activation pretreatment of rare earth concentrate

[0054] Roast bastnaesite concentrate at 500°C for 1 hour to obtain activated ore;

[0055] (2) Activated ore calcification transition pretreatment

[0056] Mix the activated ore obtained in step (1) with CaO evenly at a mass ratio of 100:100, then mix the mixture with 1.0mol / L NaOH solution at a solid-to-liquid ratio of 1kg:10L for calcification and fluorine-fixing transition pretreatment, and the transition temperature is 300°C, the transformation time is 2 hours, and then solid-liquid separation is carried out to obtain transformation slag and lye, and the lye is directly recycled;

[0057] (3) Transformation slag acid leaching

[0058] (3a) The transformation slag obtained in step (2) and 1.5mol / L hydrochloric acid solution were subjected to acid leaching treatment according to the solid-to-liquid ratio of 1kg:20L, the leaching temperature was 90°C, the leaching time was 30min, and the mass fraction added duri...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
quality scoreaaaaaaaaaa
quality scoreaaaaaaaaaa
Login to View More

Abstract

The invention belongs to the technical field of rare earth metallurgy, and particularly relates to a method for calcification transformation-leaching and decomposition of bastnaesite ore, which is carried out according to the following steps: activation pretreatment of rare earth concentrate → calcification transformation pretreatment of activated ore → acid leaching of transformation slagchlorine Rare earth semen is extracted, and finally a solution of thorium iron slag and cerium chloride, lanthanum chloride, praseodymium chloride or neodymium chloride is obtained to efficiently separate rare earth elements, fluorine elements, thorium elements and other valuable components. The invention reduces energy consumption and fuel consumption. Low-temperature roasting below 500°C only decomposes carbonate. It not only provides reactivity of rare earth concentrates, but also avoids waste of fluorine resources and emission pollution, and is a green cleaning process.

Description

technical field [0001] The invention belongs to the technical field of rare earth metallurgy, in particular to a method for decomposing bastnaesite by calcification transformation-leaching. Background technique [0002] Bastnaesite is an important rare earth resource in the world. The mineral is mainly produced in Sichuan and Shandong in China and Mountain Pass in the United States. Bastnaesite, which is rich in Sichuan, Shandong and other places, is the second largest rare earth resource in my country, and rare earths exist in the form of fluorocarbonates. After beneficiation, the concentrate grade can reach 50% to 70%, and the concentrate generally contains 8% to 9% fluorine. At present, the industrial processes for decomposing bastnaesite to extract rare earths include acid method and alkali method. [0003] Among them, the acid leaching method includes hydrochloric acid and sulfuric acid decomposition methods. In the 1990s, bastnaesite in Sichuan area of ​​my country w...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C22B59/00C22B1/02
Inventor 张廷安豆志河吕国志牛丽萍刘燕赫冀成
Owner NORTHEASTERN UNIV LIAONING
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products