Method for preparing inorganic particle/epoxy resin super hydrophobic film
A technology of epoxy resin and inorganic particles, which is applied in the field of preparation of inorganic particle/epoxy resin composite super-hydrophobic films, can solve the problems of limiting the wide application of super-hydrophobic coatings, the inability to form large-scale films, and the complexity of the preparation process. Good self-cleaning performance, simple production process, good repeatability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] (1) Preparation of aminated titanium dioxide and silica particles
[0030] Add 0.51g of titanium dioxide particles, 0.84g of silicon dioxide particles, 6.63g of γ-aminopropyltriethoxysilane and 5.61g of ammonia water into 100ml of ethanol solvent, stir and react at room temperature for 8 hours, dry and grind at 100°C to obtain Aminated titanium dioxide and silica particles;
[0031] (2) Preparation of Coating Sol
[0032] Add the amino-modified titanium dioxide and silicon dioxide particles prepared in step (1) into 35ml of ethanol solvent, then add 14g of epoxy resin, stir and react at room temperature to obtain a coating sol; the epoxy resin is selected from water-based epoxy resin ;
[0033] (3) Coating film on base material
[0034] Apply the coating sol in step (2) evenly on the glass sheet by drop coating, and let it stand at room temperature for use;
[0035] (4) Post-processing of substrate materials
[0036] Put the glass sheet coated in step (3) in...
Embodiment 2
[0038] (1) Preparation of aminated titanium dioxide and silica particles
[0039] Add 0.26g of titanium dioxide particles, 0.42g of silicon dioxide particles, 4.52g of γ-aminopropyltriethoxysilane and 3.14g of ammonia water into 100ml of ethanol solvent, stir and react at room temperature for 8 hours, dry and grind them into powder at 100°C to obtain Aminated titanium dioxide and silica particles;
[0040] (2) Preparation of Coating Sol
[0041] Add the amino-modified titanium dioxide and silicon dioxide particles prepared in step (1) into 35ml of ethanol solvent, then add 10g of epoxy resin, stir and react at room temperature to obtain a coating sol; the epoxy resin is selected from water-based epoxy resin ;
[0042] (3) Coating film on base material
[0043] Apply the coating sol in step (2) evenly on the glass sheet by drop coating, and let it stand at room temperature for use;
[0044] (4) Post-processing of substrate materials
[0045] Put the glass sheet coat...
Embodiment 3
[0047] (1) Preparation of aminated titanium dioxide and silica particles
[0048] Add 0.75g of titanium dioxide particles, 1.5g of silicon dioxide particles, 10.5g of γ-aminopropyltriethoxysilane and 8.5g of ammonia water into 120ml of ethanol solvent, stir and react at room temperature for 8 hours, dry and grind them into powder at 100°C to obtain Aminated titanium dioxide and silica particles;
[0049] (2) Preparation of Coating Sol
[0050] Add the amino-modified titanium dioxide and silicon dioxide particles prepared in step (1) to 50ml of ethanol solvent, then add 20g of epoxy resin, stir and react at room temperature to obtain a coating sol; the epoxy resin is selected from water-based epoxy resin ;
[0051] (3) Coating film on base material
[0052]Apply the coating sol in step (2) evenly on the glass sheet by drop coating, and let it stand at room temperature for use;
[0053] (4) Post-processing of substrate materials
[0054] Put the glass sheet coated in s...
PUM
Property | Measurement | Unit |
---|---|---|
size | aaaaa | aaaaa |
size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com