Preparation method for polyester fiber with composite ultraviolet, static electricity and pilling resisting functions
An anti-ultraviolet and polyester fiber technology, applied in the manufacture of conductive/anti-static filaments, fiber chemical characteristics, single-component polyester artificial filaments, etc., can solve problems such as damage, poor anti-ultraviolet performance, and easy generation of static electricity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] This embodiment provides a method for preparing an anti-ultraviolet, anti-static, anti-pilling polyester chip, which includes the following steps:
[0036] (1), primary esterification reaction section: take 18kg of purified terephthalic acid (PTA), 7.5kg of ethylene glycol (EG) and add 70 liters of polyester experimental equipment, after stirring evenly, start to heat up and pressurize to 0.3Mpa, Esterification is carried out, and the esterification temperature is controlled at 250-265°C. After the esterification is completed, the water is discharged, and the normal pressure is returned to complete the reaction.
[0037](2) Secondary esterification reaction section: After the primary esterification is completed, ethylene glycol is first added to lower the temperature of the reactor to 230-235°C, and then 450g of polyethylene glycol with a number average molecular weight of 2500 that has been heated and melted The diol was added into the reactor under the protection of n...
Embodiment 2
[0040] This embodiment provides a method for preparing an anti-ultraviolet, anti-static, anti-pilling polyester chip, which includes the following steps:
[0041] (1), primary esterification reaction section: take 18kg of purified terephthalic acid (PTA), 7.5kg of ethylene glycol (EG) and add 70 liters of polyester experimental equipment, after stirring evenly, start to heat up and pressurize to 0.3Mpa, Esterification is carried out, and the esterification temperature is controlled at 250-265°C. After the esterification is completed, the water is discharged, and the normal pressure is returned to complete the reaction.
[0042] (2) Secondary esterification reaction section: After the primary esterification is completed, ethylene glycol is first added to lower the temperature of the reactor to 230-235°C, and then 450g of polyethylene glycol with a number average molecular weight of 2500 that has been heated and melted The diol was added into the reactor under the protection of ...
Embodiment 3
[0045] This embodiment provides a method for preparing an anti-ultraviolet, anti-static, anti-pilling polyester chip, which includes the following steps:
[0046] (1), primary esterification reaction section: take 18kg of purified terephthalic acid (PTA), 7.5kg of ethylene glycol (EG) and add 70 liters of polyester experimental equipment, after stirring evenly, start to heat up and pressurize to 0.3Mpa, Esterification is carried out, and the esterification temperature is controlled at 250-265°C. After the esterification is completed, the water is discharged, and the normal pressure is returned to complete the reaction.
[0047] (2) Secondary esterification reaction section: After the primary esterification is completed, ethylene glycol is first added to lower the temperature of the reactor to 230-235°C, and then 450g of polyethylene glycol with a number average molecular weight of 3000 that has been heated and melted is added The diol was added into the reactor under the prote...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com