Embodiment 1
[0021] The weight percentages of the main elements of the wire are shown in Table 1.
[0022] Al
Mg
Ti
B
Fe+Si+Cu
Zn
15%
0.50%
0.50%
0.05%
≤1.00%
margin
[0023] preparation:
[0024] The structural schematic diagram of the horizontal continuous casting equipment adopted in the present invention is as follows: figure 1 . Among them: 1 is the heat preservation crystallization furnace; 2 is the crystallizer; 3 is the pressing roller; 4 is the pulling roller; 5 is the coiling device; 6 is the cooling water pipe;
[0025] 1) Preheat the crucible of the melting furnace to dark red, add zinc ingots with a mass fraction of 90%, then add aluminum ingots, heat and melt until the melt temperature reaches 923K or more, use a mass fraction of 0.1 ~ 0.3% of the refining agent ( In this embodiment, 0.2% zinc chloride is used for refining, the remaining zinc ingots are added, and the preheated aluminum-magn...
Embodiment 2
[0030] The difference from Example 1 is: the wire composition is: Al, 20%; RE, 0.5%; impurities, less than 1%; the balance Zn. The alloy wire wool is cast by the copper mold, the temperature of the alloy liquid in the furnace is stable at 60K higher than the melting point, the casting speed is 0.015m / s, and the cooling water pressure is 0.15×10 5 Pa, the outlet water temperature is 308K. The rough rough wire is subjected to 3.0hr homogenization annealing treatment at 513K, and then drawn and reduced to φ2.00 after 8 times of drawing. +0.00 -0.10 mm of zinc-aluminum alloy wire products, and coiled into a circle.
Embodiment 3
[0032]The difference from Example 1 is that: the composition of the wire rod is: Al, 10%; RE, 0.06%; Mg, 0.03%; impurity, less than 1%; the balance is Zn. Copper crystallizer is used to cast alloy wire wool, the alloy liquid temperature in the furnace is stable at 80K higher than the melting point, the casting speed is 0.015m / s, and the cooling water pressure is 0.12×10 5 Pa, the outlet water temperature is 308K. The rough rough wire is subjected to homogenization annealing treatment at 493K for 3.0hr.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com