Graphene modified epoxide anticorrosive coating and preparation method thereof
A technology for epoxy anti-corrosion coatings and graphene modification, which is applied in the direction of anti-corrosion coatings, epoxy resin coatings, coatings, etc. It can solve problems such as uneven grafting, restrictions on the application of graphene, and different production and application habits, and achieve dispersion good sex effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0038] The graphene-modified epoxy anticorrosion coating of this embodiment is mainly made of 60gA component and 10gB component, and described A component is mainly made of 19.2g epoxy resin 901, 16.6g titanium dioxide, 20g talcum powder, 0.6g BYK180 and 3.6 g graphene dispersion liquid composition, described B component is 10g polyamide solidifying agent, and the mass ratio of described graphene dispersion liquid and described A component is 6:100.
[0039] The graphene dispersion is obtained by compounding 20g graphene, 200g mixed solvent and 10g Lubrizol 32500, and the mixed solvent is 80g xylene, 20g cyclohexanone, 20g butanol, 50g ethylene glycol ether, and 30g ethyl ether. A mixture of glycol ether acetates.
[0040] The preparation method of the graphene modified epoxy anticorrosion coating in the present embodiment may further comprise the steps:
[0041] 1) Preparation of premixed solution: 19.2g of epoxy resin 901, 16.6g of titanium dioxide, 20g of talcum powder and...
Embodiment 2
[0048] The graphene-modified epoxy anticorrosion coating of the present embodiment is mainly made by 70gA component and 10gB component, and described A component is mainly made of 21g epoxy resin E44, 19.83g zinc phosphate, 20g barium sulfate, 0.77gAFCONA3777 and 8.4 g graphene dispersion liquid composition, described B component is 10g phenalkamine solidifying agent, and the mass ratio of described graphene dispersion liquid and described A component is 12:100.
[0049] The graphene dispersion is mainly obtained by compounding 20g graphene, 300g mixed solvent and 16g Ona F410, and the mixed solvent is 144g xylene, 32g cyclohexanone, 37g butanol, 58g ethylene glycol ether, and 29g ethyl ether. A mixture of glycol ether acetates.
[0050] The preparation method of the graphene modified epoxy anticorrosion coating in the present embodiment may further comprise the steps:
[0051] 1) Preparation of premixed solution: 21g of epoxy resin E44, 19.83g of zinc phosphate, 20g of bariu...
Embodiment 3
[0058] The graphene-modified epoxy anticorrosion coating of the present embodiment is mainly made by 80gA component and 10gB component, and described A component is mainly made of 25.2g epoxy resin E51, 20g carbon black, 25.76g mica powder, 1.04g BYK161 and 8g graphene dispersion liquid composition, described B component is 10g aliphatic amine solidifying agent, and the mass ratio of described graphene dispersion liquid and described A component is 10:100.
[0059] Described graphene dispersion liquid is compounded by 20g graphene, 400g mixed solvent and 20g Lubrizol 32500, and described mixed solvent is 150g xylene, 43g cyclohexanone, 40g butanol, 100g ethylene glycol ethyl ether and 67g ethyl alcohol A mixture of glycol ether acetates.
[0060] The preparation method of the graphene modified epoxy anticorrosion coating in the present embodiment may further comprise the steps:
[0061] 1) Preparation of premixed solution: Mix 25.2g of epoxy resin E51, 20g of carbon black, 25...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com