Embodiment 1
[0024] A heat-insulating and heat-preserving environmentally friendly corrugated cardboard, which is provided with two or more layers of corrugated paper, an insulating layer is arranged between adjacent corrugated papers, and a special adhesive is used to bond the adjacent corrugated papers and insulating layers; The above-mentioned special adhesive includes the following components in percentage terms: 80% acrylate resin, 8% zircon sand powder, 0.7% dimer acid, 5% initiator, 0.5% emulsifier, 2.3% isopropanol, antioxidant 0.7% agent, 3% stabilizer, and the balance is water.
[0025] Preferably, the initiator is a mixture of hydrogen peroxide and tert-butyl hydroperoxide, wherein the content of hydrogen peroxide is ≤40%.
[0026] A preparation process for thermal insulation and environmental protection corrugated cardboard, comprising the following steps:
[0027] 1) Add acrylic resin, zircon sand powder, antioxidant and 50% water into No. 1 mixing cylinder and stir for react...
Embodiment 2
[0034] As described in Example 1, a heat-insulating and heat-preserving environmentally friendly corrugated cardboard and its preparation process, some of the steps can also use the following processes:
[0035] The special adhesive includes the following components by percentage: 75% acrylate resin, 10% zircon sand powder, 1.1% dimer acid, 7% initiator, 0.8% emulsifier, 1.5% isopropanol, anti Oxygen agent 0.5%, stabilizer 2%, the balance is water.
[0036] In step 1), the mixing temperature is 52°C, and the heating temperature is 126°C.
[0037] In step 2), the mixing temperature is 82°C.
[0038] In step 3), the stirring speed of the first section is 280r / min, the stirring temperature is 71°C, the stirring speed of the second section is 170r / min, the stirring temperature is 42°C, and the stirring speed of the third section is 700r / min, the stirring temperature is 102°C.
[0039] In step 4), the mixing temperature is 35° C., and the stirring speed is 108 r / min.
Embodiment 3
[0041] As described in Example 1, a heat-insulating and heat-preserving environmentally friendly corrugated cardboard and its preparation process, some of the steps can also use the following processes:
[0042] The special adhesive includes the following components by percentage: 72% acrylate resin, 12% zircon sand powder, 0.5% dimer acid, 10% initiator, 0.5% emulsifier, 3% isopropanol, anti Oxygen agent 0.5%, stabilizer 1%, the balance is water.
[0043] In step 1), the mixing temperature is 71°C, and the heating temperature is 120°C.
[0044] In step 2), the mixing temperature is 89°C.
[0045] In step 3), the stirring speed of the first section is 100r / min, the stirring temperature is 81°C, the stirring speed of the second section is 300r / min, the stirring temperature is 32°C, and the stirring speed of the third section is 400r / min, the stirring temperature is 106°C.
[0046] In step 4), the mixing temperature is 30° C., and the stirring speed is 120 r / min.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com