Particle-free silver ink, preparation method thereof and transparent silver conductive film and preparation method thereof
A conductive thin film, particle-free technology, applied to conductive layers, inks, circuits, etc. on insulating carriers, can solve the problems of high sintering temperature, easy sedimentation, clogging of nozzles, etc., and achieves simple preparation steps, reduced resistance value, and saving raw materials. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0047] A particle-free silver ink, made from silver citrate, isopropylamine, methanol and butanol, the mass percent of each component is, silver citrate: 20%, isopropylamine: 14%, methanol: 40%, butanol : 26%.
[0048] A preparation method of particle-free silver ink, comprising the following steps:
[0049] (1) According to the component formula of particle-free silver ink, take raw material, wherein, foaming agent is mixed with saturated foaming agent solution;
[0050] (2) Mix liquid isopropylamine, methanol and butanol evenly, and the mixing time is 5 minutes to obtain a mixed solution;
[0051] (3) Silver citrate was added to the mixed solution, stirred at room temperature for 30 minutes until the silver citrate was completely dissolved, and filtered with a microporous membrane with a pore size of 220 nm to obtain particle-free silver ink.
[0052] The obtained particle-free silver ink is a transparent solution, does not contain any solid particles, and is stored in the...
Embodiment 2
[0058] A particle-free silver ink, prepared from a saturated solution of silver oxalate, butylamine, ethanol, amyl alcohol and sodium bicarbonate, the mass percentage of each component is, silver oxalate: 10%, butylamine: 15%, ethanol: 35% , pentanol: 35%, sodium bicarbonate saturated solution 5%.
[0059] A preparation method of particle-free silver ink, comprising the following steps:
[0060] (1) according to the component formula of particle-free silver ink, take raw material;
[0061] (2) Mix liquid butylamine, ethanol, pentanol, and saturated sodium bicarbonate solution evenly, and the mixing time is 10 minutes to obtain a mixed solution;
[0062] (3) Silver oxalate was added to the mixed solution, stirred at room temperature for 60 minutes until the silver oxalate was completely dissolved, and then filtered with a microporous membrane with a pore size of 450 nm to obtain particle-free silver ink.
[0063] The obtained particle-free silver ink is a transparent solution...
Embodiment 3
[0069] A particle-free silver ink, prepared from silver acetate, hexylamine, ethylene glycol, butanediol, butyraldehyde, polyethylene glycol and oxalic acid saturated solution, the mass percentage of each component is, silver acetate: 15%, hexyl Amine: 12%, Ethylene Glycol: 34%, Butylene Glycol: 33%, Butyraldehyde: 2%, Polyethylene Glycol: 1%, Saturated Oxalic Acid Solution: 3%.
[0070] A preparation method of particle-free silver ink, comprising the following steps:
[0071] (1) according to the component formula of particle-free silver ink, take raw material;
[0072] (2) Mix liquid hexylamine, ethylene glycol, butanediol, butyraldehyde, polyethylene glycol and saturated oxalic acid solution evenly for 20 minutes to obtain a mixed solution;
[0073] (3) Silver acetate was added to the mixed solution, stirred at room temperature for 50 min until the silver acetate was completely dissolved, and then filtered with a microporous membrane with a pore size of 450 nm to obtain pa...
PUM
Property | Measurement | Unit |
---|---|---|
viscosity | aaaaa | aaaaa |
contact angle | aaaaa | aaaaa |
surface tension | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com