Automobile interior trim part material and preparation method thereof
A technology for automotive interiors and raw materials, applied in scratch-resistant polypropylene special materials for automotive interiors and its preparation, materials for automotive interiors and its preparations, achieving superior scratch resistance, simple preparation methods, and suitable for industrialization The effect of mass production
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0043] Example 1 Preparation of 1# anti-scratch polypropylene special material for automotive interior parts: according to the following formula, the material is prepared according to the following formula:
[0044] 75% copolymerized polypropylene;
[0045] 22.4% talc;
[0046] 0.5% POSS modified polysiloxane elastomer;
[0047] 0.5% Oleamide;
[0048] 0.5% light stabilizer Tinuvin 770;
[0049] 0.1% antioxidant 1010;
[0050] 0.1% Antioxidant 168;
[0051] 0.2% calcium hardate;
[0052] 0.7% toner.
[0053] The selected copolymerized PP is Shanghai Petrochemical PP M700R, the melt flow rate of this product is 7.0±1.8g / 10min, and the low-temperature conversion temperature of thermal properties is ≥150°C. The selected talcum powder is produced in Haicheng, Liaoning, and the particle size range is 2.5-13.5 microns. POSS modified polysiloxane elastomer is used as the anti-scratch agent, wherein the molecular weight of the polysiloxane elastomer is 600,000, POSS is TriS...
Embodiment 2
[0055] Example 2 2# Preparation of scratch-resistant polypropylene special material for automotive interior parts: in parts by mass, prepare materials according to the following formula:
[0056] 75% copolymerized polypropylene;
[0057] 21.4% talc;
[0058] 1.5% TriSilanolPhenyl POSS modified polysiloxane elastomer;
[0059] 0.5% ethylene bisstearamide (EBS);
[0060] 0.5% light stabilizer Tinuvin 770;
[0061] 0.1% antioxidant 1010;
[0062] 0.1% Antioxidant 168;
[0063] 0.2% zinc stearate;
[0064] 0.7% toner.
[0065] The addition of the above-mentioned TriSilanolPhenyl POSS modified polysiloxane elastomer is 1.5wt%; the above-mentioned raw materials are put into a high-speed mixer and fully mixed; the fully mixed compound is sent into a twin-screw extruder, and the The aspect ratio of the twin-screw extruder is 40:1, and the working temperature of the twin-screw extrusion is 160°C in the first zone, 200°C in the second zone, 210°C in the third zone, 210°C in the...
Embodiment 3
[0066] Example 3 Preparation of 3# scratch-resistant polypropylene special material: according to the mass parts, the material is prepared according to the following formula:
[0067] 75% copolymerized polypropylene;
[0068] 20.4% talc;
[0069] 2.5% TriSilanolPhenyl POSS modified polysiloxane elastomer;
[0070] 0.5% ethylene bisstearamide (EBS);
[0071] 0.5% light stabilizer Tinuvin 770;
[0072] 0.1% antioxidant 1010;
[0073] 0.1% Antioxidant 168;
[0074] 0.2% zinc stearate;
[0075] 0.7% toner.
[0076] The addition amount of the above-mentioned trisilanol isobutyl silsesquioxane (TriSilanolIsobutyl-POSS) modified polysiloxane elastomer is 2.5wt%; the above-mentioned raw materials are put into a high-speed mixer and fully mixed; the fully mixed The compounded materials are fed into the twin-screw extruder, the length-to-diameter ratio of the twin-screw extruder is 40:1, and the working temperature of the twin-screw extrusion is 160°C in the first zone, 200°C i...
PUM
Property | Measurement | Unit |
---|---|---|
melt flow index | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com