Elastomer plastic, conductive plastic, conductive plastic bipolar plate and preparation methods thereof
A technology of elastomeric plastics and conductive plastics, applied in the field of elastomeric plastics, can solve the problems of processing and tissue damage, processing and assembly damage, high electrical conductivity, etc., achieve continuous industrial production, improve long-term stability, and improve comprehensive performance. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment
[0086] 1. Preparation of elastomeric plastics
[0087] Example 1-1. The dried polypropylene pellets PP (MI-5) and PP (MI-20) (obtained from Sinopec) with a melt index (MI) of 5g / 10min and 20g / 10min respectively : After mixing with a mass ratio of 80, it is transferred to the XHM-140 internal mixer (produced by Dalian Rubber Machinery Factory), mixed and internalized at 180°C for 10 minutes, and then passed through the STJ-78 / 180 twin-screw extruder (Lanzhou Lanzhou Produced by Tai Plastic Machinery Co., Ltd.) extrusion granulation, the obtained granules are represented by EP1-1.
[0088] Example 1-2. The dried polyethylene pellets PE (MI-10) and PE (MI-30) (obtained from Sinopec) with a melt index (MI) of 10g / 10min and 30g / 10min respectively After mixing at a mass ratio of 60, it is transferred to the XHM-140 internal mixer (produced by Dalian Rubber Machinery Factory), mixed and internalized at 140°C for 10 minutes, and then passed through the STJ-78 / 180 twin-screw extruder (Lanz...
Embodiment 3-1、3-4、3-7 and 3-10
[0112] Specific process parameters of Examples 3-1, 3-4, 3-7 and 3-10
[0113] High speed mixing
[0114] Speed: 1500rmp / min
[0115] Chamber temperature: 170℃
[0116] Stirring time 30min
[0117] Extrusion granulation
[0118] The temperature of the back section of the extruder is 150℃, the temperature of the middle section is 160℃, and the outlet temperature is 165℃
[0119] Speed 15rmp / min
[0120] Mixer temperature 170℃
[0121] Twin screw extruded into tablets
[0122] The temperature of the back section of the extruder is 140℃, the temperature of the middle section is 150℃, and the outlet temperature is 155℃
[0123] Speed 10rmp / min
[0124] Cooling temperature: 30℃ water cooling.
Embodiment 3-2
[0125] Specific process parameters of Examples 3-2, 3-5, 3-8 and 3-11
[0126] High speed mixing
[0127] Speed: 1300rmp / min
[0128] Chamber temperature: 160℃
[0129] Stirring time 20min
[0130] Extrusion granulation
[0131] The temperature of the back section of the extruder is 180°C, the temperature of the middle section is 160°C, and the outlet temperature is 175°C
[0132] Speed 20rmp / min
[0133] Internal mixer temperature 160℃
[0134] Twin screw extruded into tablets
[0135] The temperature of the back section of the extruder is 120℃, the temperature of the middle section is 150℃, and the outlet temperature is 155℃
[0136] Speed 12rmp / min
[0137] Cooling temperature: 25℃ water cooling.
[0138] Specific process parameters of Examples 3-3, 3-6, 3-9 and 3-12
[0139] High speed mixing
[0140] Speed: 1400rmp / min
[0141] Chamber temperature: 130℃
[0142] Stirring time 15min
[0143] Extrusion granulation
[0144] The temperature of the back section of the extruder is 120℃, the temper...
PUM
Property | Measurement | Unit |
---|---|---|
length | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
width | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology