A technology of tung tree and flooring, which is applied in wood treatment, wood processing equipment, impregnated wood, etc. It can solve the problems of short growth period and soft material, and achieve the effects of not easy to deform and crack, increase density, and protect the ecological environment
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
example 1
[0014] Example 1. The artificial fast-growing tung tree log is sawed into 1000 * 150 * 28 (mm) slab blanks, and then soaked in a clear water pool until the water content reaches 100%.
[0015] Finally, put the slab blank into an airtight container for high-temperature cooking, degrease and soften, and then pre-dry until the water content is below 20%.
[0016] Then put the pre-dried slab into the hot press for heating and compression, so that the slab is gradually dried and densified. According to the technical requirements of the material, the slab is dried to a moisture content of 12% and densified to a compression rate of 30%. , and then turn off the hot steam, inject cooling water into the hot press plate, so that the plate blank is cooled and shaped.
[0017] Finally, unload the shaped slabs from the hot press, apply waterproofing agent on the surrounding and both sides of the slabs, stack them neatly, and regain moisture for ten days. The process is made into tung modif...
example 2
[0018] Example two. The artificial fast-growing tung tree log is sawed into a slab stock of 1000 * 120 * 32 (mm), and then soaked in a clear water pool until the water content reaches 90%.
[0019] Finally, put the plank blank into an airtight container for high-temperature cooking, and after degreasing and softening, perform pre-drying treatment until the moisture content is below 20%.
[0020] Then put the pre-dried slab into the hot press for heating and compression, so that the slab is gradually dried and densified. According to the technical requirements of the material, the slab is dried to a moisture content of 10% and densified to a compression rate of 40%. , and then turn off the hot steam, inject cooling water into the hot press plate, so that the plate blank is cooled and shaped.
[0021] Finally, unload the shaped slab blank from the hot press, apply waterproofing agent on the surrounding and both sides of the slab blank, stack it neatly, and regain moisture for 12...
example 3
[0022] Example three. The artificial fast-growing tung tree log is sawed into 1000 × 100 × 36 (mm) slab stock, and then soaked in a clear water pool until the water content reaches 80%.
[0023] Finally, put the slab blank into an airtight container for high-temperature cooking, degrease and soften, and then pre-dry until the moisture content is below 20%.
[0024] Then put the pre-dried slab into the hot press for heating and compression, so that the slab is gradually dried and densified. According to the technical requirements of the material, the slab is dried to a moisture content of 8% and densified to a compression rate of 50%. ,. Then turn off the hot steam, and inject cooling water into the hot pressing plate to cool and shape the blank.
[0025] Finally, unload the shaped slabs from the hot press, apply waterproofing agent on the surrounding and both sides of the slabs, stack them neatly, and regain moisture for 15 days. After the internal stress of the slabs is deter...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com