A kind of anti-corrosion coating and environmental protection technology, applied in anti-corrosion coatings, epoxy resin coatings, coatings and other directions, can solve the problems of poor compatibility of mechanical processing performance resin, affecting the anti-corrosion performance of polyaniline, unable to achieve anti-corrosion effect, etc. Good adhesion, high hardness and compact structure

Inactive Publication Date: 2009-08-05
SHANDONG UNIV
View PDF3 Cites 9 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] Although polyaniline has excellent anti-corrosion properties, its mechanical processing properties and compatibility with resins are poor, which limits its use.
Now the conventional methods of combining polyaniline with resin mainly include: ①Dissolution method: use a special solvent to dissolve and add it to the resin. This method will cause environmental pollution, poor construction conditions, and the expensive solvent will increase the cost sharply; : as the ball milling method, it consumes a large amount of energy and time, and its dispersion and stability in the resin are poor, which finally affects the performance of polyaniline's anticorrosion performance; (3) first dissolve polyaniline in amine curing agent, and then mix Oxygen resin compounding, this method has insurmountable defects: the content of polyaniline is low, and the content with the best anti-corrosion effect cannot be achieved

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0023] Embodiment 1: prepare a kind of anticorrosion coating, step is as follows:

[0024] (1) Preparation of Component A: The used raw material parts for the preparation of Component A are as follows:

[0025] ① Liquid epoxy resin E56 40 grams;

[0026] ② Diethylene glycol dibenzoate 4 grams;

[0027] ③OP-10 0.5g;

[0028] ④ 6 grams of n-pentanol;

[0029] ⑤ 3 grams of ammonium persulfate;

[0030] ⑥ 1.5 grams of distilled water;

[0031] ⑦1 gram of 0.4mol / L aqueous solution of camphorsulfonic acid;

[0032] ⑧4 grams of aniline;

[0033] ⑨Methicone 0.5g;

[0034] ⑩ Neopentyl glycol diglycidyl ether 4 grams.

[0035] Under nitrogen protection, add liquid epoxy resin E56, plasticizer diethylene glycol dibenzoate, OP-10, 0.9g n-pentanol (as co-emulsifier), distilled water, Ammonium sulfate was stirred rapidly for 2 hours to form a stable microemulsion system with epoxy resin and plasticizer as the oil phase and an aqueous solution of oxidant ammonium persulfate as the n...

Embodiment 2

[0039] Embodiment 2: prepare a kind of anticorrosion coating, step is as follows:

[0040] (1) Preparation of Component A: The used raw material parts for the preparation of Component A are as follows:

[0041] ① Liquid epoxy resin E42 80 grams;

[0042] ② 16 grams of dibutyl phthalate;

[0043] ③OP-10 4 grams;

[0044] ④ 10 grams of isopropanol;

[0045] ⑤ 12 grams of ammonium persulfate;

[0046] ⑥ 3 grams of distilled water;

[0047] 7. 2 grams of 0.6mol / L aqueous solution of camphorsulfonic acid;

[0048] ⑧ 16 grams of aniline;

[0049] ⑨Simethicone oil 1g;

[0050] ⑩ Propylene carbonate 4 grams.

[0051] Under nitrogen protection, add liquid epoxy resin E42, plasticizer dibutyl phthalate, emulsifier OP-10, 1.5g isopropanol (as co-emulsifier), distilled water, Ammonium sulfate was stirred rapidly for 2 hours to form a stable microemulsion system with epoxy resin and plasticizer as the oil phase and an aqueous solution of oxidant ammonium persulfate as the nucleus. T...

Embodiment 3

[0055] Embodiment 3: prepare a kind of anticorrosion coating, step is as follows:

[0056] (1) Preparation of Component A: The used raw material parts for the preparation of Component A are as follows:

[0057] ① Liquid epoxy resin E44 60 grams;

[0058] ② Dioctyl phthalate 10 grams;

[0059] ③OP-10 2.5g;

[0060] ④ 8 grams of n-butanol;

[0061] ⑤ 4 grams of ammonium persulfate;

[0062] ⑥ 2 grams of distilled water;

[0063] 7. 0.5 grams of 0.8mol / L aqueous solution of camphorsulfonic acid;

[0064] ⑧ 6 grams of aniline;

[0065] ⑨Methicone 0.8g;

[0066] ⑩ Neopentyl glycol diglycidyl ether 4 grams.

[0067] Under nitrogen protection, add liquid epoxy resin E44, plasticizer dioctyl phthalate, emulsifier OP-10, 1.2g n-butanol (as co-emulsifier), distilled water, Ammonium sulfate was stirred rapidly for 3 hours to form a stable microemulsion system with epoxy resin and plasticizer as the oil phase and an oxidant aqueous solution as the core. The system was placed in a...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses environmental-friendly anti-corrosive polyaniline paint which has high content of polyaniline, good anti-corrosion performance and low cost, causes no pollution and is suitable for preventing steel, magnesium and other metals from being corroded. The environmental-friendly anti-corrosive polyaniline paint contains component A and component B which have the weight ratio of 7:1 to 17:1, wherein the component A contains the following components according to the portion by weight: 40-80 portions of liquid epoxy resin, 4-40 portions of plasticizing agent, 0.1-4 portion(s) of emulsifying agent OP-10, 4-10 portions of small-molecular fatty alcohol, 0.1-15 portion(s) of ammonium persulfate, 0.1-3 portion(s) of distilled water, 0.1-2 portion(s) of 0.4-0.8mol / L camphorsulfonic acid solution, 0.1-16 portion(s) aniline, 0.5-1 portion of defoaming agent and 4-20 portions of reactive diluent.

Description

technical field [0001] The invention relates to an environment-friendly polyaniline anticorrosion coating and a preparation method thereof. Background technique [0002] The loss caused by metal corrosion to human beings is staggering. According to statistics, the annual metal loss caused by corrosion in the world is as high as 20%-40% of the global metal production, and the economic loss is about 1 trillion US dollars. Practice has proved that the use of coatings for corrosion protection of metals is the most economical, practical and effective method. However, the current commonly used anti-corrosion coatings contain a large amount of organic solvents, which cause great pollution to the environment during the construction process and pose a huge threat to the health of workers; at the same time, commonly used anti-corrosion coatings are also rich in zinc, which not only consumes a lot of zinc resources, but also affects the health of workers. The environment is seriously ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): C09D5/08C09D163/02C09D179/02
Inventor 石元昌徐晓脍王颖刘峰陈辉
Owner SHANDONG UNIV
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products