A technology for coal tar and diesel oil, which is applied in the processing of tar by distillation method and tar refining by chemical method, etc., can solve the problems of hydrogenation catalyst activity, unfavorable hydrothermal stability and strength, catalyst deactivation, catalyst coke deposition, etc. , to achieve the effect that the production technology is easy to master, the process is simple, and the equipment investment is small.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0022] Catalyst component: Y type molecular sieve 50g contains potassium iodide 0.8g aqueous solution 30ml;
[0023] Preparation method: impregnating the Y-type molecular sieve with an aqueous solution of potassium iodide for 2 hours, and drying at a temperature of 120°C for 2 hours to obtain a catalyst, the properties of which are shown in Table 1;
[0024] Utilize above-mentioned catalyst to carry out coal tar to produce diesel oil:
[0025] Add 300g of coal tar with a water content of 1wt% to the 1000ml autoclave device, and then add 4.5g of catalyst. After the autoclave is sealed, heat the autoclave to raise the temperature to 350°C, keep the temperature for 5 minutes, and then drop to room temperature Finally, the reaction product is taken out from the reactor, and then separated by distillation, and the fraction at 80-280°C is taken to obtain diesel oil; see Table 2 for the properties of diesel oil.
[0026] Potassium iodide in the catalyzer of the present embodiment is...
Embodiment 2
[0028] Catalyst component: ZSM-5 molecular sieve 50g contains potassium iodide 0.8g aqueous solution 25ml;
[0029] Preparation method: ZSM-5 molecular sieve was impregnated with an aqueous solution of potassium iodide for 2 hours, and dried at a temperature of 120° C. for 2 hours to obtain a catalyst whose properties are shown in Table 1;
[0030] Utilize above-mentioned catalyst to carry out coal tar to produce diesel oil:
[0031] Add 300g of coal tar with a moisture content of 0.1wt% to the 1000ml autoclave device, and then add 4.5g of catalyst. After the reactor is sealed, heat the reactor to raise the temperature to 360°C, keep the temperature for 10 minutes, and then drop to room temperature Finally, the reaction product is taken out from the reactor, and then separated by distillation, and the fraction at 80-280°C is taken to obtain diesel oil; see Table 2 for the properties of diesel oil.
[0032] Potassium iodide in the catalyzer of the present embodiment is 1.21% o...
Embodiment 3
[0034] Catalyst component: γ-Al 2 o 3 50g 30ml of aqueous solution containing 1.0g of potassium iodide;
[0035] Preparation method: γ-Al 2 o 3 Immerse in an aqueous solution of potassium iodide for 2 hours and dry for 1 hour at a temperature of 120°C to obtain a catalyst whose properties are shown in Table 1;
[0036] Utilize above-mentioned catalyst to carry out coal tar to produce diesel oil:
[0037] Add 300g of coal tar with a water content of 1.8wt% to the 1000ml autoclave device, and then add 4.5g of catalyst. After the reactor is sealed, heat the reactor to raise the temperature to 350°C, keep the temperature for 15 minutes, and then drop to room temperature Finally, the reaction product is taken out from the reactor, and then separated by distillation, and the fraction at 80-280°C is taken to obtain diesel oil; see Table 2 for the properties of diesel oil.
[0038] Potassium iodide in the catalyzer of the present embodiment is 1.66% of catalyzer weight in terms ...
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
dew point | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com