A kind of protective liquid, nano technology, applied in textile and papermaking, fiber processing, fiber type and other directions, can solve problems such as relatively high processing conditions, unsatisfactory waterproof effect, limited application scope of protective liquid, etc., to achieve a wide range of suitable Applicable, accessible, easy-to-apply effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0049] A kind of nano protective liquid for weaving, its composition comprises (by weight percentage):
[0050] (1) Nano silicon oxide 0.5%
[0051] (2) Tridecafluorooctyltriethoxysilane 1%
[0052] (3) Fluoroalkyl acrylate 5%
[0053] (4) Deionized water 93.5%
[0054] Preparation:
[0055] (1) First, 10 grams of 60nm nano-silicon oxides in the components of the present invention are evenly dispersed in 40 grams of deionized water to prepare 50 grams of stable dispersions with a concentration of 20%;
[0056] (2) Then 50 grams of the stable dispersion liquid prepared in step (1) was added to 1830 grams of deionized water and mixed with 20 grams of tridecafluorooctyltriethoxysilane and 100 grams of fluoroalkyl acrylate Evenly, the nano protective solution is prepared.
[0057] Instructions:
[0058] (1) Before the nano-protection liquid of the present invention is processed to the fabric, it is necessary to thoroughly wash off oil stains, dust, etc. with clear water, and...
Embodiment 2
[0061] A kind of nano protective liquid for weaving, its composition comprises (by weight percentage):
[0062] (1) Nano titanium oxide 1%
[0063] (2) Trifluoropropyltrimethoxysilane 1%
[0064] (3) Fluoroalkyl acrylate 4%
[0065] (4) Deionized water 94%
[0066] Preparation:
[0067] (1) First, 15 grams of nano-titanium oxide of 50nm level in the components of the present invention are uniformly dispersed in 35 grams of deionized water to obtain a stable dispersion with a concentration of 30%;
[0068] (2) Then 50 grams of the stable dispersion liquid prepared in step (1) is added to 1375 grams of deionized water and mixed with 15 grams of trifluoropropyltrimethoxysilane and 60 grams of fluoroalkyl acrylate and stirred evenly A nano protective solution is prepared.
[0069] Instructions:
[0070] (1) Before the nano-protection liquid of the present invention is processed to the fabric, it is necessary to thoroughly wash off oil stains, dust, etc. with clear water, an...
Embodiment 3
[0073] A kind of nano protective liquid for weaving, its composition comprises (by weight percentage):
[0074] (1) Nano alumina 0.1%
[0075] (2) Propyltrimethoxysilane 5%
[0076] (3) Fluoroalkyl acrylate 8%
[0077] (4) Deionized water 86.9%
[0078] Preparation:
[0079] (1) First, 5 grams of 10nm nano-alumina in the components of the present invention are uniformly dispersed in 45 grams of deionized water to obtain a stable dispersion with a concentration of 10%;
[0080] (2) Then add 50 grams of the stable dispersion prepared in step (1), 250 grams of propyltrimethoxysilane, and 400 grams of fluoroalkyl acrylate to 4300 grams of deionized water, mix and stir evenly to obtain Nano protective fluid.
[0081] Instructions:
[0082] (1) Before the nano-protection liquid of the present invention is processed to the fabric, it is necessary to thoroughly wash off oil stains, dust, etc. with clear water, and the newly bought clothes are treated in the same way;
[0083] (...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com