A technology for thermal insulation materials and walls, applied in the field of building materials, can solve the problems of high thermal conductivity, poor fire resistance, complicated construction, etc., and achieve the effects of low moisture content and water absorption, good thermal insulation, and easy promotion of construction.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0033] Weigh 12.5 kg of magnesium oxide or magnesium hydroxide, 5 kg of magnesium chloride, 6.5 kg of perlite, 2.5 kg of straw fiber, 8 kg of fly ash or calcium carbonate, and 0.5 kg of modifier, wherein the modifier is composed of the following weight ratios: Serving composition:
[0034] 8 parts ferrous sulfate
[0035] oxalic acid 2 parts
[0036] Trisodium Phosphate 2 parts
[0037] Six bias 1 part
[0038] Aluminum sulfate 15 parts
[0039] It is also possible to add polyphenylene particles accounting for 1 to 5% of the total weight, and dissolve the above-mentioned magnesium chloride and modifier into water to make the concentration reach 17 to 25%; then add magnesium oxide, perlite, straw fiber, fly ash or carbonic acid Add calcium to the solution in the step (the weight ratio of the two is 1:1), stir evenly and form a paste material, apply the paste material to the construction wall within 30 minutes, and add magnesium oxide by weight 5% water repellent in solutio...
Embodiment 2
[0041] Weigh 10 kg of magnesium oxide or magnesium hydroxide, 3 kg of magnesium chloride, 5 kg of perlite, 3 kg of straw fiber, 10 kg of fly ash or calcium carbonate, and 0.8 kg of modifier, wherein the modifier is composed of the following weight ratios: Serving composition:
[0042] 6 parts ferrous sulfate
[0043] 3 parts oxalic acid
[0044] Trisodium Phosphate 1 part
[0045] Six bias 1.5 parts
[0046] Aluminum sulfate 16 parts
[0047] Above-mentioned magnesium chloride and modifying agent are melted into water, make its concentration reach 17~25%, then magnesium oxide, perlite, straw fiber, fly ash or calcium carbonate are added in the solution of step (the weight ratio position of both is 0.5: 1) Stir evenly to form a paste, and apply the paste to the construction wall within 30 minutes. In addition, a waterproofing agent with a weight of 5% magnesium oxide can be added to the solution.
Embodiment 3
[0049] Weigh 15 kg of magnesium oxide or magnesium hydroxide, 5 kg of magnesium chloride, 8 kg of perlite, 5 kg of straw fiber, 8 kg of fly ash or calcium carbonate, and 0.3 kg of modifier, wherein the modifier is composed of the following weight ratios: Serving composition:
[0050] 10 parts ferrous sulfate
[0051] 1 part oxalic acid
[0052] Trisodium Phosphate 3 parts
[0053] Six bias 2 copies
[0054] Aluminum sulfate 17 parts
[0055] Above-mentioned magnesium chloride and modifying agent are melted into water, and its concentration reaches 19%, then magnesium oxide, perlite, straw fiber, fly ash or calcium carbonate are added in the solution of step (the weight ratio position of both is 0.8: 1) , Stir evenly and form a paste material, which can be applied to the construction wall within 30 minutes. In addition, a waterproofing agent with a weight of 5% magnesium oxide can be added to the solution.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com