Sulfuric acid resistant pure austenitic stainless steel welding rod with high nickel-copper content and low hot cracking sensitivity and preparation method
An austenitic stainless steel, crack-sensitive technology, applied in welding equipment, welding medium, manufacturing tools, etc., can solve the problems of high price, changes in structure and performance, etc., and achieve high thermal crack resistance, excellent elongation, The effect of welding arc stabilization
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0042] Take 100kg of nickel-chromium-molybdenum-copper-iron alloy welding core, the composition of nickel-chromium-molybdenum-copper-iron alloy welding core is (wt%): C 0.03%, Mn2.35%, Si 0.25%, Cr 20.55%, Ni 34.02%, the sum of Nb and Ta 0.28%, Cu 3.58%, Mo 2.81%, S0.002%, P 0.002%, Sn 0.007%, Sb 0.004%, As 0.006%, and the balance is Fe and essential impurities.
[0043] Take the drug skin, the weight of each component in the drug skin is as follows: containing TiO 2 94wt% rutile powder 12kg; contains CaCO 3 98.50wt% marble powder 5.0kg; containing CaF 2 97.3wt% fluorite powder 1.5kg; containing SiO 2 55wt%, Al 2 o 3 3.6kg of 32.5wt% mica powder; containing SiO 2 60.8wt%, Al 2 o 3 15.2wt%, K 2 O+Na 2 O 19.6wt% potassium feldspar powder 2.8kg; Mn 99.5wt% electrolytic manganese 2.8kg; Nb 99.75wt% niobium powder 0.5kg; Cr 98wt% metal chromium powder 1.3kg; Mo 55wt% molybdenum Iron powder 0.35kg; containing Na 2 CO 3 98.5wt% soda ash 0.3kg; containing Na 2 O11.5wt% so...
Embodiment 2
[0047] The welding rod of this embodiment is all the same as that of Embodiment 1 except that the weight of each component in the coating is different.
[0048] In the present embodiment, the weight of each component in the medicine skin is as follows: containing TiO 2 94wt% rutile powder 8kg; containing CaCO 3 6.5kg of 98.50wt% marble powder; containing CaF 2 97.3wt% fluorite powder 3kg; containing SiO 2 55wt%, Al 2 o 3 3.6kg of 32.5wt% mica powder; containing SiO 2 60.8wt%, Al 2 o 3 15.2wt%, K 2 O+Na 2 O 19.6wt% potassium feldspar powder 2.5kg; Mn 99.5wt% electrolytic manganese 2.4kg; Nb 99.75wt% niobium powder 0.3kg; Cr 98wt% metal chromium powder 1.8kg; Mo 55wt% molybdenum Iron powder 0.45kg; containing Na 2 CO 3 98.5wt% soda ash 0.3kg; containing Na 2 O 11.5wt% sodium alginate 0.2kg;
[0049] The obtained sulfuric acid corrosion-resistant pure austenitic stainless steel electrode 2 with high nickel and copper content and low thermal crack sensitivity was sub...
Embodiment 3
[0051] The welding rod of this embodiment is all the same as that of Embodiment 1 except that the weight of each component in the coating is different.
[0052] In the present embodiment, the weight of each component in the medicine skin is as follows: containing TiO 2 94wt% rutile powder 8kg; containing CaCO 3 7kg of 98.50wt% marble powder; containing CaF 2 97.3wt% fluorite powder 3kg; containing SiO 2 55wt%, Al 2 o 3 32.5wt% mica powder 2.0kg; containing SiO 2 60.8wt%, Al 2 o 3 15.2wt%, K 2 O+Na 2 O 19.6wt% potassium feldspar powder 2.2kg; Mn99.5wt% electrolytic manganese 2.8kg; Nb 99.75wt% niobium powder 0.3kg; Cr 98wt% metal chromium powder 1.8kg; Mo 55wt% molybdenum Iron powder 0.55kg; containing Na 2 CO 3 98.5wt% soda ash 0.3kg; containing Na 2 O 11.5wt% sodium alginate 0.2kg;
[0053] The resulting sulfuric acid corrosion-resistant pure austenitic stainless steel electrode 3 with high nickel and copper content and low thermal crack sensitivity was subjecte...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com