A kind of method for preparing porous cerium oxide catalytic material
A catalytic material, cerium oxide technology, applied in chemical instruments and methods, metal/metal oxide/metal hydroxide catalysts, physical/chemical process catalysts, etc., can solve the problems of oxygen detachment, surface oxygen vacancy defects, porosity Advanced problems, to achieve the effect of efficient transformation, simple synthesis process and low cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] Mix 10g of cerium nitrate hexahydrate (10g including the mass of water in the hydrate, the same below), 30g of water, 30g of ethanol, 5g of citric acid, and 5g of glycerin in a beaker, stir well, and heat and stir in an oil bath at 100°C Until the material is gel-like and foaming, the foamed material is dried in an oven at 80°C for 24 hours, and then fired in a muffle furnace at 600°C for 3 hours to obtain a porous cerium oxide airgel with high porosity .
[0022] Add 400 mg of the above catalyst into 4.6 g of toluene, fill with 2.5 MPa oxygen, react at 160° C. for 24 hours, the conversion rate is 50.1%, and the selectivity of benzaldehyde and benzyl alcohol is >99%.
Embodiment 2
[0024] Mix 10g of cerium chloride heptahydrate, 30g of water, 30g of ethanol, 5g of citric acid, and 5g of glycerin in a beaker, stir evenly, place in an oil bath at 100°C and heat and stir until the material becomes gelatinous and foams. The foamed material was dried in an oven at 80°C for 24h, and then calcined in a muffle furnace at 600°C for 3h to obtain a porous cerium oxide airgel with high porosity.
[0025] Add 400 mg of the above catalyst into 4.6 g of toluene, fill with 2.5 MPa oxygen, react at 160° C. for 24 hours, the conversion rate is 39.2%, and the selectivity of benzaldehyde and benzyl alcohol is >99%.
Embodiment 3
[0027] Mix 10g of cerium acetate pentahydrate, 30g of water, 30g of ethanol, 5g of citric acid, and 5g of glycerin in a beaker, stir evenly, place in an oil bath at 100°C and heat and stir until the material is gelatinous and foaming. The foamed material was dried in an oven at 80°C for 24h, and then calcined in a muffle furnace at 600°C for 3h to obtain a porous cerium oxide airgel with high porosity.
[0028] Add 400 mg of the above catalyst into 4.6 g of toluene, fill with 2.5 MPa oxygen, react at 160° C. for 24 hours, the conversion rate is 46.6%, and the selectivity of benzaldehyde and benzyl alcohol is >99%.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com