Inorganic fusion cake for tempered glass inkjet printing ink and automotive tempered glass inkjet printing ink prepared from inorganic fusion cake
An inkjet printing, tempered glass technology, applied in glass manufacturing equipment, glass tempering, ink and other directions, can solve the problems of low ink covering power, unable to reach automotive tempered glass, etc., and achieve high acid resistance.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0069] An inorganic frit of tempered glass inkjet printing ink, calculated as 100% by its total weight percentage, comprises the following components:
[0070] 25% SiO 2 , 15% ZnO, 10% Bi 2 o 3 , 20% B 2 o 3 , 10%K 2 O, 10% Na 2 O, 5% ZrO 2 , 1% Li 2 O, 1%TiO 2 , 3%V 2 o 5 .
[0071] A glass inkjet printing ink prepared by using the above-mentioned inorganic frit, calculated according to its total weight percentage as 100%, includes the following components:
[0072] Inorganic frit: 20%, organic solvent: 65%, dispersant: 1%, antistatic agent: 0.1%, copper chrome black: 13.9%.
[0073] The dispersant is Solsperse 20000, and the antistatic agent is CHEMSTAT3500.
[0074] Based on the total weight percentage of the organic solvent as 100%, it includes the following components calculated in weight percentage: isopropanol: 48.6%, butyl acetate: 11%, cyclohexanone: 24%, diethylene glycol monobutyl Ether: 11.4%, petroleum ether 5%.
[0075] The steps of preparing the a...
Embodiment 2
[0084] An inorganic frit of tempered glass inkjet printing ink, calculated as 100% by its total weight percentage, comprises the following components:
[0085] 45% SiO 2 , 30% ZnO, 15% Bi 2 o 3 , 5% B 2 o 3 , 1%K 2 O, 1% Na 2 O, 1% Li 2 O. 0.1%V 2 o 5 ;1.9%TiO 2 .
[0086] A glass inkjet printing ink prepared by using the above-mentioned inorganic frit, calculated according to its total weight percentage as 100%, includes the following components:
[0087] Inorganic frit: 60%; organic solvent: 35%; dispersant: 1%; antistatic agent: 0.1%, copper chrome black: 3.9%.
[0088] The dispersant is Solsperse 20000, and the antistatic agent is CHEMSTAT3500.
[0089] Based on the total weight percentage of the organic solvent as 100%, it includes the following components calculated in weight percentage: cyclohexanone: 24%; dipropylene glycol methyl ether: 48.6%; propylene glycol diacetate: 12%; diethylene glycol Alcohol monobutyl ether: 10.4%; Petroleum ether: 5%.
[0090...
Embodiment 3
[0099] An inorganic frit of tempered glass inkjet printing ink, calculated as 100% by its total weight percentage, comprises the following components:
[0100] 30% SiO 2 , 20% ZnO, 30% Bi 2 o 3 , 10% B 2 o 3 , 1.5%K 2 O, 2% Na 2 O, 2%TiO 2 , 2%Li 2 O, 2.5%V 2 o 5 .
[0101] A glass inkjet printing ink prepared by using the above-mentioned inorganic frit, calculated according to its total weight percentage as 100%, includes the following components:
[0102] Inorganic colored frit: 25%; organic solvent: 45%; dispersant: 15%; antistatic agent: 4.5%; copper chrome black: 10.5%.
[0103] The dispersant is 0.7% Solsperse 8000 and 0.3% DISPERBYK-163; the antistatic agent is JWK-200, and the organic solvent is ethylene glycol.
[0104] The specific steps of manufacturing the glass inkjet printing ink of this embodiment are as follows:
[0105] 1. Weigh the components of the above-mentioned inorganic frit according to weight percentage and mix them evenly, then place them...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com