A method for comprehensive recovery of arsenic-containing materials and arsenic resource utilization
A technology of resource utilization and materials, applied in the field of metallurgy, can solve the problems of untreated sodium arsenate, low recovery rate of valuable metals, complicated pH adjustment process, etc., to improve the quality of recovered products, high comprehensive utilization of resources, and adaptability to raw materials. wide range of effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0043] Taking arsenic-containing soot from a lead-zinc smelter in China as an example, the main components of the raw materials are Pb 1.57%, As48.56%, Sn0.51%, Sb 21.24%, Zn 0.73%, Te 0.35%, Se 0.25%, and the following steps are adopted deal with:
[0044] (1) Oxygen pressure water immersion: Weigh a certain quality of high arsenic and antimony fumes into the reactor, the control conditions are liquid-solid volume mass ratio 10:1, stirring speed 300r / min, leaching temperature 160°C, oxygen partial pressure 2Mpa, The leaching time is 2 hours. After the leaching is completed and the oxidation blowing temperature is 700°C, the slurry is removed and separated by filtration to obtain the leaching solution and leaching residue;
[0045] After testing: the arsenic leaching rate is 61.53%, and the concentration of each element in the leach solution is Pb 709.60ppm, Se31.02ppm, Sb1.26g / L, Te 123.28ppm, As 29.88g / L.
[0046] (2) Selective reduction and purification of leach solution: ...
Embodiment 2
[0053] Taking arsenic-containing soot from a lead-zinc smelter in China as an example, the main components of the raw material are Pb 6.88%, As36.51%, Sn1.11%, Sb 29.77%, Zn 0.54%, Te 0.24%, Se 0.05%, and the following steps are adopted deal with:
[0054] (1) Oxygen pressure water immersion: Weigh a certain quality of high arsenic and antimony fumes into the reactor, the control conditions are liquid-solid volume mass ratio 20:1, stirring speed 300r / min, leaching temperature 160°C, oxygen partial pressure 0.5Mpa , the leaching time is 2h, after the leaching is completed and the oxidation blowing temperature is 800°C, the slurry is removed and separated by filtration to obtain the leachate and leach residue;
[0055] After testing: the arsenic leaching rate is 51.29%, and the concentration of each element in the leach solution is Pb 515.20ppm, Se31.56ppm, Sb0.88g / L, Te 122.26ppm, As 9.36g / L.
[0056] (2) Selective reduction and purification of the leach solution: under the co...
Embodiment 3
[0063] Taking arsenic-containing soot from a lead-zinc smelter in China as an example, the main components of the raw material are Pb 5.46%, As 30.29%, Sn0.98%, Sb 29.58%, Zn 0.68%, Te 0.26%, Se 0.07%, and the following steps are used for processing :
[0064] (1) Oxygen pressure water immersion: Weigh a certain quality of high arsenic and antimony fume in the reaction kettle, the control conditions are liquid-solid volume mass ratio 10:1, stirring speed 300r / min, leaching temperature 200℃, oxygen partial pressure 2.5Mpa , the leaching time is 4h, after the leaching is completed and the oxidation blowing temperature is 650°C, the slurry is removed and separated by filtration to obtain the leachate and leach residue;
[0065] After testing: the arsenic leaching rate is 64.52%, and the concentration of each element in the leach solution is Pb 956.35ppm, Se18.91ppm, Sb0.93g / L, Te 144.92ppm, As 19.54g / L.
[0066] (2) Selective reduction and purification of the leach solution: at ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com