Embodiment 1
[0030] The preparation process of the present embodiment group horn glue is as follows:
[0031] 1. Preparation of component I: mixing temperature 70-75°C, premixing time 1 hour, vacuum mixing 3 hours.
[0032] a. Preheat the polyol for 12-16 hours at 70-80°C;
[0033] b. The filler is dried and dehydrated for 18-20 hours at 200°C;
[0034] c. Feeding (double planetary power mixer A)
[0035] Trifunctional polyether polyol (M=1000) 36.7kg
[0036] Two-functional polyether polyol (M=1000) 7.2kg
[0037] 5000 mesh heavy calcium carbonate 30.35kg
[0038] Nano calcium carbonate 8kg
[0039] Polyether polyol (M=300) 7kg
[0040] Organic Bismuth 0.05kg
[0041] Silicone oil 1kg
[0042] Petroleum ether (T50) 3.2kg
[0043] Potassium hydrogen phthalate 6.5kg
[0044] 2. Preparation of component II: mixing temperature 70-75°C, premixing time 1 hour, vacuum mixing 3 hours.
[0045] a. Preheat the medium molecular weight trifunctional polyether polyol for 12-16 hours at 70-8...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com