Water-based anti-corrosion paint
An anti-corrosion coating, water-based technology, applied in the direction of anti-corrosion coatings, epoxy resin coatings, coatings, etc., can solve the problems of destroying the ecological environment of water bodies, the decrease of dissolved oxygen content in water, and the deterioration of water quality, so as to achieve anti-corrosion and protection. Anode, anti-flash rust effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] The water-based anticorrosion paint of the present invention comprises the following components by weight,
[0021] Bisphenol A / F type epoxy resin 40
[0022] Polyamidoamine 50
[0023] Calcium borosilicate 8
[0024] Titanium dioxide 3
[0026] Mica 8
[0027] Deionized water 100
[0028] The calcium borosilicate salt is mixed with calcium carbonate, silicon dioxide, and boric acid in a mass ratio of 4:5:1 for 24 hours, then placed in a platinum crucible and melted at 1350-1500 degrees Celsius for 0.5-2 hours, poured Quenching into deionized water to form borosilicate calcium salt fragments, using an ultrasonic crusher to grind through a 100-mesh sieve to obtain borosilicate calcium salt powder.
Embodiment 2
[0030] The water-based anticorrosion paint of the present invention comprises the following components by weight,
[0031] Bisphenol A / F type epoxy resin 45
[0032] Polyamidoamine 55
[0033] Calcium borosilicate 9
[0034] Titanium dioxide 4
[0036] mica 9
[0037] Deionized water 100
[0038] The calcium borosilicate salt is mixed with calcium carbonate, silicon dioxide, and boric acid in a mass ratio of 4:5:1 for 24 hours, then placed in a platinum crucible and melted at 1350-1500 degrees Celsius for 0.5-2 hours, poured Quenching into deionized water to form borosilicate calcium salt fragments, using an ultrasonic crusher to grind through a 100-mesh sieve to obtain borosilicate calcium salt powder.
Embodiment 3
[0040] The water-based anticorrosion paint of the present invention comprises the following components by weight,
[0041] Bisphenol A / F type epoxy resin 50
[0042] Polyamidoamine 60
[0043] Calcium borosilicate 10
[0044] Titanium dioxide 5
[0045] Barium sulfate 10
[0046] Mica 10
[0047] Deionized water 100
[0048] The calcium borosilicate salt is mixed with calcium carbonate, silicon dioxide, and boric acid in a mass ratio of 4:5:1 for 24 hours, then placed in a platinum crucible and melted at 1350-1500 degrees Celsius for 0.5-2 hours, poured Quenching into deionized water to form borosilicate calcium salt fragments, using an ultrasonic crusher to grind through a 100-mesh sieve to obtain borosilicate calcium salt powder.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com