Electroplating process of electroplated metal fastener
An electroplating process and a technology of electroplating metal, which are applied in the field of electroplating technology, can solve the problems of slow electroplating deposition speed and weak bonding of electroplating layers, and achieve the effects of fast electroplating deposition speed, strong corrosion resistance, and firm bonding of electroplating layers
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] Example 1 Electroplated Metal Fasteners
[0023] Copper-plated, nickel-plated and zinc-plated on the surface of the metal base of the screw in sequence, the steps are as follows:
[0024] (1) Solution composition and process conditions of copper electroplating process: copper sulfate 135 mg / L, malic acid 90 mg / L, citric acid 210 mg / L, potassium citrate 40 mg / L, sodium hypophosphite 20 mg / L, Glucose 15 mg / L; current density 1.5A / dm 2 , the anode is 3‰ phosphorus-containing copper plate, the area ratio of anode and cathode is 2:1, the temperature is 20-25°C, and the time is 8 minutes;
[0025] (2) Solution composition and process conditions of electroplating nickel process: sodium hydroxide 100mg / L, nickel chloride 15mg / L, sodium chloride 60mg / L, phosphorous acid 85mg / L, succinic acid 40mg / L, methylol Acrylic acid 110mg / L, boric acid 175mg / L, sodium dodecylbenzenesulfonate 20mg / L; current density is 3A / dm 2 , the anode is made of stainless steel, the temperature is 70°...
Embodiment 2
[0030] Example 2 Electroplated Metal Fasteners
[0031] Copper-plated, nickel-plated and zinc-plated on the surface of the metal base of the screw in sequence, the steps are as follows:
[0032](1) Solution composition and process conditions of copper electroplating process: copper sulfate 120mg / L, malic acid 100 mg / L, citric acid 200 mg / L, potassium citrate 50 mg / L, sodium hypophosphite 10mg / L, glucose 20 mg / L; the current density is 1A / dm 2 , the anode is 3‰ phosphorus-containing copper plate, the area ratio of anode and cathode is 2:1, the temperature is 25°C, and the time is 10 minutes;
[0033] (2) Solution composition and process conditions of electroplating nickel process: sodium hydroxide 80mg / L, nickel chloride 25mg / L, sodium chloride 50mg / L, phosphorous acid 90mg / L, succinic acid 30mg / L, methylol Acrylic acid 120mg / L, boric acid 150mg / L, sodium dodecylbenzenesulfonate 30mg / L; current density is 2A / dm 2 , the anode is made of stainless steel, the temperature is 80°...
Embodiment 3
[0038] Example 3 Electroplated Metal Fasteners
[0039] Copper-plated, nickel-plated and zinc-plated on the surface of the metal base of the screw in sequence, the steps are as follows:
[0040] (1) Solution composition and process conditions of copper electroplating process: copper sulfate 150 mg / L, malic acid 80 mg / L, citric acid 220 mg / L, potassium citrate 30 mg / L, sodium hypophosphite 30 mg / L, Glucose 10 mg / L; current density 2A / dm 2 , the anode is 3‰ phosphorus-containing copper plate, the area ratio of anode and cathode is 2:1, the temperature is 20°C, and the time is 8 minutes;
[0041] (2) Solution composition and process conditions of electroplating nickel process: sodium hydroxide 120mg / L, nickel chloride 10mg / L, sodium chloride 70mg / L, phosphorous acid 80mg / L, succinic acid 50mg / L, methylol Acrylic acid 100mg / L, boric acid 200mg / L, sodium dodecylbenzenesulfonate 10mg / L; current density is 5A / dm 2 , the anode is made of stainless steel, the temperature is 60°C, an...
PUM
Property | Measurement | Unit |
---|---|---|
Current density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com