[0021] 1. Preparation of photosensitive polymer:
[0022] 1. Preparation of macromolecular photosensitizer:
[0023] Add an appropriate amount of 2,4 dihydroxybenzophenone (UV-0) and a weight ratio of 0.8%~2% NaOH into a dry three-necked flask, fill with nitrogen for 30 minutes, then add glycidyl methacrylate ( GMA), (the molar ratio to UV-0 is 1:1~2:1), stir and heat up to 60°C~90°C, and the reaction time is 3h~8h, to obtain a yellow viscous liquid (BPMA), keep away from light for use ;
[0024] 2. Preparation of hydrophilic photosensitive polymer:
[0025] Add the polymer monomers N-vinylpyrrolidone (VP) and BPMA into the three-necked flask respectively (the amount of VP and BPMA can account for 10%~90% of the total moles of the two), add an appropriate amount of deionized water, and add Sodium dodecyl sulfate (SDS) with a weight ratio of 1%~10%, adding 1%~5% azobisisobutylcyanide (AIBN) as an initiator, nitrogen gas for 30 minutes, stirring, reflux, and reaction temperat...
Embodiment 1
[0036] 1. Preparation of photosensitive polymer:
[0037] 1. Preparation of macromolecular photosensitizer:
[0038] Add 10.7g of 2,4 dihydroxybenzophenone (UV-0) and 0.155g of NaOH into a dry three-necked flask, fill with nitrogen for 30 minutes, then add 7.9g of glycidyl methacrylate (GMA), (with UV The molar ratio of -0 is 1:1), and the temperature was raised to 80°C with stirring, and the reaction time was 5 hours to obtain a yellow viscous liquid (BPMA), which was kept away from light for use.
[0039] 2. Preparation of photosensitive polymer:
[0040] To 33g N-vinylpyrrolidone (VP) and 12gBPMA (wherein the amount of VP and BPMA accounts for 90% and 10% of the total moles of the two respectively) in the three-necked flask, add an appropriate amount of deionized water, and the weight ratio is 1.7g ( 4wt% sodium dodecyl sulfate (SDS), add 0.48g (2wt%) azobisisobutylcyanide (AIBN), blow nitrogen for 30 minutes, stir, reflux, reaction temperature 80°C, reaction time 3h. Af...
Embodiment 2
[0045] 1. Preparation of photosensitive polymer:
[0046] 1. Preparation of macromolecular photosensitizer:
[0047] Add 10.7g of 2,4 dihydroxybenzophenone (UV-0) and 0.212g of NaOH into a dry three-necked flask, fill with nitrogen for 30 minutes, then add 15.8g of glycidyl methacrylate (GMA), (with UV The molar ratio of -0 is 2:1), and the temperature was raised to 60°C with stirring, and the reaction time was 3 hours to obtain a yellow viscous liquid (BPMA), which was kept away from light for use.
[0048] 2. Preparation of photosensitive polymer:
[0049] Add 3.7g of N-vinylpyrrolidone (VP) and 108g of BPMA to the three-necked flask respectively (the amount of VP and BPMA accounted for 10% and 90% of the total moles of the two respectively), and add an appropriate amount of deionized water at a weight ratio of 1.17g (1wt%) sodium dodecyl sulfate (SDS), add 1.17g (1wt%) ammonium persulfate (APS), blow nitrogen for 30 minutes, stir, reflux, reaction temperature 50°C, reacti...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com