Light ecological concrete brick and preparation method thereof
An eco-concrete, light-weight technology, applied in the field of water treatment, can solve the problem that the effectiveness cannot be maintained for a long time, and achieve the effect of reducing the overall density, reducing the sludge content, and not easy to lose
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0047] Prepare the microbial mixed bacterium powder according to the following method:
[0048] (1) Bacterial strain collection: the soil, water, silt in saline-alkali land, coastal tidal flat areas, and activated sludge from sewage treatment plants are used as samples for collecting bacterial strains.
[0049] (2) Separation and screening: using the coating method or the mixed bacteria method, through the three steps of plate inoculation, streak separation and purification, the samples containing bacillus, nitrifying bacteria, photosynthetic bacteria and actinomycetes are directional isolated from the collected samples. , yeast, and lactic acid bacteria flora; then inoculate the above six flora into triangular flasks filled with artificially simulated sewage, respectively use a constant temperature shaker to cultivate the aerobic bacteria in each flora, and use a constant temperature incubator to stand still. The anaerobic bacteria in each flora are cultured in a closed manne...
Embodiment 2
[0054] Prepare lightweight ecological concrete bricks (type A) (30 bricks) as follows:
[0055] (1) Get 1 kg of the mixed microbial bacterial powder prepared in Example 1, premix it with 1.2 kg of water for 5 hours, and configure it as a mixed microbial bacterial liquid;
[0056] (2) Combine the above-mentioned mixed microbial bacterial liquid with 20kg of cement, 5.6kg of perlite, and 0.2kg of sawdust to form a base material, and stir evenly for about 5 minutes;
[0057] (3) Add the stirred base material into the mould, and press down on the mould's upper head for 5 seconds to obtain a semi-finished brick;
[0058] (4) Harden the semi-finished bricks in a natural state for 7 days to obtain 30 finished lightweight ecological concrete bricks (Type A).
Embodiment 3
[0060] Prepare lightweight ecological concrete bricks (type B) (30 bricks) as follows:
[0061] (1) Get 2kg of the mixed microbial bacterial powder prepared in Example 1, premix it with water 1.2kg for 5 hours, and configure it as a mixed microbial bacterial liquid;
[0062] (2) Combine the above-mentioned mixed microbial bacterial liquid with 20kg of cement, 2.8kg of perlite, 50kg of gravel, and 0.2kg of wood chips to form a base material, and stir evenly for about 5 minutes;
[0063] (3) Add the stirred base material into the mould, and press down on the mould's upper head for 5 seconds to obtain a semi-finished brick;
[0064] (4) Harden the semi-finished bricks in a natural state for 7 days to obtain 30 finished lightweight ecological concrete bricks (type B).
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com