A coating and water-based technology, which is applied in the field of water-based anti-corrosion coating with rust and its preparation, can solve the problems of increased cost, time-consuming and laborious, and incomplete rust treatment, and achieve excellent weather resistance and salt spray resistance. Construction Convenience, excellent effect of weather resistance and salt spray resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] Weigh the components according to the following masses:
[0027] Epoxy resin E-44 22.5g
[0028] Barite 12g
[0029] Titanium Dioxide 11g
[0030] Talc 12g
[0031] Aradur3986 50g
[0032] Deionized water 48.5g
[0033] Aluminum tripolyphosphate 10g
[0036] Iron oxide red 7.5g
[0037] CX-500 1.76g
[0038] Tributyl Phosphate 0.2g
[0039] The preparation process is as follows:
[0040] 12g of barite, 11g of titanium dioxide, 12g of talc, 50g of water-based epoxy curing agent, 16g of deionized water, 10g of aluminum tripolyphosphate, 10g of zinc phosphate, 5g of zinc powder and 7.5g of red iron oxide, CX-5001.76 g Put it in a high-speed blender and mix well. Then add 22.5g of liquid epoxy resin E-4444, 0.2g of tributyl phosphate, continue to stir, add 32.5g of deionized water to dilute to required viscosity after mixing evenly, to obtain the water-based epoxy resin coating.
Embodiment 2
[0042] Weigh the components according to the following masses:
[0043] Epoxy resin E-54 22.5g
[0044] Barite 12g
[0045] Titanium Dioxide 11g
[0046] Talc 12g
[0047] Aradur3986 50g
[0048] Deionized water 48.5g
[0049] Aluminum tripolyphosphate 10g
[0051] Zinc powder 5g
[0052] Iron oxide red 7.5g
[0053] CX-500 1.76g
[0054] Tributyl Phosphate 0.2g
[0055] The preparation process is as follows:
[0056] Put 12g of barite, 11g of titanium dioxide, 12g of talc, 50g of Aradur3986, 16g of deionized water, 10g of aluminum tripolyphosphate, 10g of zinc phosphate, 5g of zinc powder, 7.5g of iron oxide red, and 1.76g of CX-500 respectively. Mix well in a high-speed mixer. Then add 22.5 g of liquid epoxy resin E-54 and 0.2 g of tributyl phosphate, continue to stir, add 32.5 g of deionized water after mixing evenly, and dilute to the required viscosity to obtain the water-based epoxy resin coating.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com