Wood-plastic composite material and prepration method thereof
A technology of wood-plastic composite materials and plastics, applied in the field of wood-plastic materials containing lignocellulose materials and its preparation, can solve the problems of weak strength and poor compatibility of wood-plastic composite materials, and achieve bending strength and impact strength Enhanced, increased compatibility, and resource-saving effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0071] 1. Prepare materials according to the following proportions by weight:
[0072] Modified Fiber Powder 70
[0073] HDPE 30
[0074] Maleic anhydride grafted polyethylene 4
[0075] Polyethylene Wax 6
[0076] Antioxidant 264 0.2
[0078] Ammonium Polyphosphate 2
[0079] Among them, the molecular weight of high density polyethylene (HDPE) is 40000-300000, and the density is 0.94g / cm 3 , the melt index (MI, g / 10min) is 0.35; the molecular weight of maleic anhydride grafted polyethylene is 10000-300000, the graft ratio is 1.5%, the melt index is 0.5g / 10min; the molecular weight of polyethylene wax is 2500-3000, Density 0.92g / cm 3 , the viscosity is 0.8Pa·s (140℃); the nitrogen content of ammonium polyphosphate is 23%, and the phosphorus content is ≥20%.
[0080] Wherein, the modified fiber powder is prepared according to the following steps:
[0081] A. After the poplar is pulverized into 40 mesh wood powder with a wood flour machine ...
Embodiment 2
[0092] 1. Prepare materials according to the following proportions by weight:
[0093] Modified Fiber Powder 65
[0094] Polypropylene 35
[0095] Maleic anhydride grafted polypropylene 5
[0096] Stearic acid 6
[0097] Antioxidant 264 0.1
[0098] Antioxidant 1010 0.1
[0100] Octabromoether flame retardant 2
[0101] Wherein, the molecular weight of the polypropylene (PP) is 10000-300000, the melt index (MI, g / 10min) is 0.4; the molecular weight of the maleic anhydride grafted polypropylene is 12000-300000, the graft ratio is 2%, Melt index 0.6g / 10min.
[0102] Wherein, the modified fiber powder is prepared according to the following steps:
[0103] A. After the masson pine wood is pulverized into 100 mesh wood powder by a wood powder machine, the wood powder is placed in a desiccator and dried at 105 ° C to obtain dry pine fiber powder, wherein the moisture content of the dry pine fiber powder is 5% ;
[0104] B, dry wood powder and li...
Embodiment 3
[0109] 1. Prepare materials according to the following proportions by weight:
[0110] Modified fiber powder 80
[0111] PVC 20
[0112] Rare Earth Composite Stabilizer 5
[0113] Stearic acid 3
[0114] Rosin 3
[0115] Chlorinated polyethylene 6
[0116] Antioxidant 264 0.1
[0117] Antioxidant 1010 0.2
[0119] Chlorinated paraffin flame retardant 2.5
[0120] Wherein, the molecular weight of the polyvinyl chloride (PVC) is 30000-100000, the melt index (MI) is 0.8g / 10min; the molecular weight of the chlorinated polyethylene is 10000-300000, and the chlorine content is 40%; The molecular weight is 1060-1100, and the chlorine content is 70%; the rare earth metal content in the rare earth composite stabilizer is more than 10%, the moisture content is less than 2%, and the particle size is more than 200 mesh.
[0121] Wherein, the modified fiber powder is prepared according to the following steps:
[0122] A. After pulverizing Chinese fir...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
melt flow index | aaaaa | aaaaa |
melt flow index | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com