A wear-resistant cast iron and high-chromium technology, applied in the field of wear-resistant metal materials, can solve the problems of high production cost of high-chromium cast iron, decreased toughness of high-chromium cast iron, and increased number of carbides, etc., and achieves improved hardenability and excellent wear resistance. The effect of stability and performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0040] ① Mix steel scrap, ferrochrome and pig iron into the furnace to heat and melt, add ferrosilicon and ferromanganese after the molten iron is melted;
[0041] ② After adjusting the ingredients in front of the furnace, raise the temperature to 1560-1600°C, add silicon-calcium alloy for pre-deoxidation; after 1-2 minutes of pre-deoxidation, add aluminum for final deoxidation; After adding 1 to 2 minutes, add ferroboron; add ferroboron for 1 to 2 minutes and take it out of the oven;
[0042] ③Crush the barium-silicon alloy, strontium-silicon alloy and lanthanum-cerium mixed rare earth into small pieces with a particle size of 4-10mm. After drying at 150-180°C, place them at the bottom of the ladle, and use the method of pouring into the ladle to degrade the molten iron. deal with;
[0043] ④Pouring molten iron into castings, the temperature of molten iron pouring is 1420~1480℃;
[0044] ⑤ Normalize the casting at 980°C, hold for 6 hours, and finally temper at 250°C, hold f...
Embodiment 2
[0046] Steps ①~④ are the same as Steps ①~④ in Example 1;
[0047] ⑤ Normalize the casting at 1050°C, hold for 4 hours, and finally temper at 500°C, hold for 8 hours to obtain boron-containing high-chromium wear-resistant cast iron. The chemical composition is shown in Table 1, and the mechanical properties are shown in Table 2.
Embodiment 3
[0049] Steps ①~④ are the same as Steps ①~④ in Example 1;
[0050] ⑤ Normalize the casting at 1000°C, hold for 5 hours, and finally temper at 450°C, hold for 9 hours to obtain boron-containing high-chromium wear-resistant cast iron. The chemical composition is shown in Table 1, and the mechanical properties are shown in Table 2.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com