A hydrogenation catalyst and catalyst technology, applied in the direction of selective hydrorefining, etc., can solve the problems of undescribed hydrogenation of styrene and its derivatives, easy polymerization, and high reaction temperature, so as to improve hydrogenation activity and anti-glue The effect of good ability, activity and anti-colloid ability, and simple preparation process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] Use pseudo-thin water aluminum hydroxide powder containing 62% alumina (the rest is water) to make small balls with a diameter of 2-5mm. After drying at 120°C for 3 hours, raise the temperature to 600°C in normal pressure air. ℃, keep the temperature for 2 hours, feed water vapor, the volume ratio of water vapor and air is 50%, keep the temperature for another 2 hours under this condition, then stop the water vapor, and continue roasting in the air at 600 ℃ for 3 hours. After being impregnated with a nickel nitrate solution containing 120 g / l of nickel for 3 hours, it is filtered, dried at 80-90° C. for 15 hours, and calcined at 480° C. for 4 hours. The impregnation was repeated one more time to achieve the desired high nickel content, and the drying and firing conditions were the same as above.
[0025] The prepared catalyst composition is: NiO: 28.5%, Al 2 o 3 : 71.5%. Specific surface area: 180 meters 2 / g, pore volume: 0.46 ml / g, the pore volume of pores larger ...
Embodiment 2
[0028] Use pseudo-thin water aluminum hydroxide powder containing 70% alumina (the rest is water) to make small balls with a diameter of 2-5mm. After drying at 110°C for 4 hours, raise the temperature to 630°C in normal pressure air. ℃, keep the temperature for 1 hour, feed water vapor, the volume ratio of water vapor and air is 80%, keep the temperature for another 2 hours under this condition, then stop the water vapor, and continue roasting at 650 ℃ in the air for 2 hours. A nickel nitrate solution containing 130 g / l of nickel is used, impregnated for 4 hours, filtered, dried at 90-100° C. for 10 hours, and roasted at 350° C. for 5 hours.
[0029] The prepared catalyst composition is: NiO: 19.6%, Al 2 o 3 : 80.4%. Specific surface area: 150 meters 2 / g, pore volume: 0.65 ml / g, the pore volume of pores larger than 5nm accounts for 93% of the total pore volume, and the most probable pore diameter is 15nm.
[0030] Catalyst performance evaluation: See Table 1 for the proper...
Embodiment 3
[0032] Use pseudo-thin water aluminum hydroxide powder containing 75% of alumina (the rest is water) to make small balls with a diameter of 2-5mm. After drying at 100°C for 5 hours, raise the temperature to 660°C in normal pressure air. ℃, constant temperature for 1 hour, feed water vapor, the volume ratio of water vapor and air is 30%, keep the temperature for another 2 hours under this condition, then stop the water vapor, and continue roasting in air at 680°C for 2 hours. A nickel nitrate solution containing 150 g / l of nickel is used, impregnated for 5 hours, filtered, dried at 110-120° C. for 8 hours, and roasted at 400° C. for 3 hours.
[0033] The prepared catalyst composition is: NiO: 12.5%, Al 2 o 3 : 87.5%. Specific surface area: 110 meters 2 / g, pore volume: 0.82 ml / g, the pore volume of pores larger than 5nm accounts for 95% of the total pore volume, and the most probable pore diameter is 19nm.
[0034] Catalyst performance evaluation: The raw material oil used ...
PUM
Property | Measurement | Unit |
---|---|---|
specific surface area | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com