Wax emulsion for treating pencil wood
A wax emulsion, wood technology, applied in the direction of wood impregnation, wood impregnation, wood processing equipment, etc., can solve the problems of rough cutting surface, not solving the difficulty of cutting the finished pen, and achieve smooth cutting surface, easy cutting, and reduce environmental pollution. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] 6% paraffin wax No. 52;
[0032] 9% montan wax;
[0033] 5% stearic acid;
[0034] 6% hydroxyethyl ethylenediamine triacetic acid;
[0035] 6% sorbitan monooleate;
[0036] 1% borax;
[0037] water, balance.
[0038] According to the ratio of Example 1, the materials other than water were taken and added to the stainless steel reactor, slowly heated to 110°C, stirred and mixed for 10 minutes, then added hot water at 90°C under high-speed stirring to mix, disperse and emulsify, keep it constant for 20 minutes, and then After homogenizer treatment, it is the wax emulsion of the present invention.
Embodiment 2
[0040] 8% No. 54 paraffin;
[0041] 11% montan wax;
[0042] 6% vegetable oleic acid;
[0043] 7% oxalic acid;
[0044] 8% polyoxyethylene (20) sorbitan tristearate;
[0045] 2% sodium benzoate;
[0046] water, balance.
[0047] According to the ratio of Example 2, materials other than water were taken and added to the stainless steel reactor, slowly heated to 105°C, stirred and mixed for 10 minutes, then added hot water at 85°C under high-speed stirring to mix, disperse and emulsify, keep it constant for 20 minutes, and then After homogenizer treatment, it is the wax emulsion of the present invention.
Embodiment 3
[0049] 14% No. 56 paraffin;
[0050] 7% montan wax;
[0051] 7% hydroxyethyl ethylenediamine triacetic acid;
[0052] 8% stearic acid;
[0053] 4% polyoxyethylene (20) sorbitan tristearate;
[0054] 1% fatty alcohol polyoxyethylene ether (A-20);
[0055] 1% borax;
[0056] water, balance.
[0057] According to the ratio of Example 3, materials other than water were taken and added to the stainless steel reactor, slowly heated to 115°C, stirred and mixed for 10 minutes, then added hot water at 95°C under high-speed stirring to mix, disperse and emulsify, keep it constant for 20 minutes, and then After homogenizer treatment, it is the wax emulsion of the present invention.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com