Environmentally-friendly wood preservative and preparation method thereof
A wood preservative and environmentally friendly technology, applied in the fields of botanical equipment and methods, wood treatment, impregnating wood, etc., can solve the problems of wood preservative, mildew proof, insect proof and rain proof that cannot be guaranteed, and reduce labor and material costs. The effect of low consumption, simple preparation process and easy production
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] Materials: single- and double-chain quaternary ammonium salts (Golden), cetyl amine oxide (Golden), paraffin (Tianshi), imidacloprid, ethylene glycol, cyproconazole and deionized water.
[0022] Preparation:
[0023] (1) Prepare 30 parts of single- and double-chain quaternary ammonium salts, 10 parts of cyclaconazole, 30 parts of paraffin, 2 parts of imidacloprid, 8 parts of ethylene glycol, 10 parts of cyclaconazole and 10 parts of water;
[0024] (2) Mix the ethylene glycol and water evenly to obtain a mixed solution; wherein, the mixing speed is 80r / min, and the mixing time is 5min;
[0025] (3) Add the single- and double-chain quaternary ammonium salts, cetyl amine oxide, and cyclaconazole into the mixed solution, and mix evenly at a stirring speed of 80 r / min;
[0026] (4) Slowly add the paraffin wax emulsion into the above mixed solution, reduce the stirring speed to 30r / min, and mix for 25min. Obtain described novel environment-friendly wood preservative.
Embodiment 2
[0028] Materials: single- and double-chain quaternary ammonium salts (Golden), cetyl amine oxide (Golden), paraffin (Tianshi), imidacloprid, ethylene glycol, cyproconazole and deionized water.
[0029] Preparation:
[0030] (1) Prepare 25 parts of single- and double-chain quaternary ammonium salts, 10 parts of cetylamine oxide, 30 parts of paraffin, 2 parts of imidacloprid, 10 parts of ethylene glycol, 8 parts of cyproconazole and 15 parts of water;
[0031] (2) Mix the ethylene glycol and water evenly to obtain a mixed solution; wherein, the mixing speed is 80r / min, and the mixing time is 5min;
[0032] (3) Add the quaternary ammonium salt, cetyl amine oxide, and cyclaconazole into the mixed solution, and mix evenly at a stirring speed of 80 r / min.
[0033] (4) Slowly add the paraffin wax emulsion into the above mixed solution, reduce the stirring speed to 30r / min, and mix for 25min. Obtain described novel environment-friendly wood preservative.
Embodiment 3
[0035] Materials: single- and double-chain quaternary ammonium salts (Golden), stearyl amine oxide (Golden), paraffin (Tianshi), dinotefuran, 1,2-propylene glycol, tebuconazole and deionized water.
[0036] Preparation:
[0037] (1) Prepare 30 parts of single- and double-chain quaternary ammonium salts, 10 parts of stearyl amine oxide, 26 parts of paraffin, 1 part of dinotefuran, 10 parts of 1,2-propanediol, 8 parts of tebuconazole and 15 parts of water;
[0038] (2) Mix the 1,2-propanediol and water evenly to obtain a mixed liquid; wherein, the mixing speed is 80r / min, and the mixing time is 5min;
[0039] (3) Add the single- and double-chain quaternary ammonium salts, stearylamine oxide, dinotefuran, and tebuconazole into the mixed solution, and mix evenly at a stirring speed of 80r / min;
[0040] (4) Slowly add the paraffin wax emulsion into the above mixed solution, reduce the stirring speed to 30r / min, and mix for 25min. Obtain described novel environment-friendly wood p...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com