A technology of modified asphalt and asphalt materials, which is applied in building insulation materials, building components, buildings, etc., can solve problems such as structural instability, poor storage stability, construction, etc., to reduce the amount of SBS and improve interface compatibility , the effect of reducing production costs
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] A kind of high-viscosity modified asphalt material, described high-viscosity modified asphalt is made of 100 parts of base asphalt, 4 parts of SBS (YH-792), 10 parts of 30 mesh waste rubber powder, 5 parts of aromatic hydrocarbon oil, 1 part of phthalate Dioctyl formate, 0.2 parts of sulfur, 2 parts of terpene resins, 1.5 parts of polyphosphoric acid and 0.7 parts of polypropylene glycol, the specific preparation steps are as follows:
[0027] (1) 100 parts of base asphalt is heated to 160°C.
[0028] (2) Premixing: first slowly add 5 parts of aromatic oil, and then use a mechanical stirrer to stir for 5 minutes to fully mix the base asphalt and aromatic oil; then slowly add 4 parts of SBS (YH-792) and keep the temperature at 160°C Stir at low temperature for 5 minutes; slowly add 10 parts of 30 mesh waste rubber rubber powder while stirring until the mixture is uniform without obvious particles, then keep stirring at 160°C for 5 minutes; then slowly add 2 parts of terp...
Embodiment 2
[0036] A kind of high-viscosity modified asphalt material, described high-viscosity modified asphalt is by 100 parts of matrix pitches, 7 parts of SBS (YH-792), 4 parts of EVA, 4 parts of aromatic hydrocarbon oils, 0.2 part of sulfur, 4 parts of terpene resins, 3 parts of dibutyl phthalate, 0.5 part of polyphosphoric acid, and 0.2 part of polypropylene glycol. The specific preparation steps are as follows:
[0037] (1) 100 parts of base asphalt is heated to 165°C.
[0038] (2) Premixing: first slowly add 4 parts of aromatic oil, and then use a mechanical stirrer to stir for 10 minutes while adding, so that the base asphalt and aromatic oil are fully mixed; then slowly add 7 parts of SBS (YH-792), and keep the temperature at 160 ° C Stir at low temperature for 10 minutes; slowly add 4 parts of EVA while stirring until the mixture is uniform and without obvious particles, then keep stirring at 160°C for 10 minutes; then slowly add 4 parts of terpene resin while stirring, and sti...
Embodiment 3
[0045] A kind of high-viscosity modified asphalt material, described high-viscosity modified asphalt is made of 100 parts of base asphalt, 5.5 parts of SBS (YH-792), 7 parts of waste rubber powder, 3 parts of aromatic hydrocarbon oil, 2 parts of sulfur-containing stabilizer 3 Part of terpene resin, 2 parts of dibutyl phthalate, 0.9 part of polyphosphoric acid, 0.45 part of polypropylene glycol composition, concrete preparation steps are as follows:
[0046] (1) 100 parts of base asphalt is heated to 165°C.
[0047] (2) Premixing: first slowly add 3 parts of aromatic oil, and then use a mechanical stirrer to stir for 8 minutes to fully mix the base asphalt and aromatic oil; then slowly add 5.5 parts of SBS (YH-792) and keep the temperature at 160°C Stir at low temperature for 8 minutes; slowly add 7 parts of waste rubber powder while stirring until the mixture is uniform and without obvious particles, then keep stirring at 160°C for 8 minutes; then slowly add 3 parts of terpene...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com