Novel energy-saving brick and processing technology thereof
A processing technology and technology of energy-saving bricks, applied in the field of building materials, can solve the problems of low breaking strength, not smooth surface, easy to be corroded, etc., and achieve the effect of environmental protection, easy decomposition, and not easy to break.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] A new energy-saving brick and its processing technology. The weight ratio of the new energy-saving brick is: 250 parts of Portland cement, 650 parts of sand, 20 parts of expanded perlite, 70 parts of cinder, 20 parts of aluminum alloy, and 3 parts of straw , 5 parts of plant ash, 6 parts of thickening powder, 5 parts of deodorant additive, and 175 parts of clear water.
[0029] In the present invention, gallic tannic acid is used as the deodorizing aid, wherein the content of gallic tannic acid is 56%.
[0030] A new type of energy-saving brick processing technology, the production steps are as follows:
[0031] (1) Weigh and mix the raw materials. First, mix the Portland cement, sand, expanded perlite, cinder, aluminum alloy, straw, plant ash, thickened powder and water according to the weight parts, and stir evenly. First, the silicate Mix cement, sand, expanded perlite and cinder into clean water to make a mixture, then add aluminum alloy, straw, plant ash and thick...
Embodiment 2
[0039] A new energy-saving brick and its processing technology. The weight ratio of the new energy-saving brick is: 200 parts of Portland cement, 710 parts of sand, 15 parts of expanded perlite, 50 parts of cinder, 10 parts of aluminum alloy, and 6 parts of straw , 3 parts of plant ash, 5 parts of thickening powder, 2 parts of deodorant additive, 140 parts of clear water.
[0040] In the present invention, gallic tannic acid is used as the deodorizing aid, wherein the content of gallic tannic acid is 78%.
[0041] A new type of energy-saving brick processing technology, the production steps are as follows:
[0042] (1) Weigh and mix the raw materials. Firstly, Portland cement, sand, expanded perlite, cinder, aluminum alloy, straw, plant ash, thickened powder and clear water are evenly mixed according to weight parts, and evenly stirred. First, silicic acid Mix salt cement, sand, expanded perlite and cinder into clean water to make a mixture, then add aluminum alloy, straw, pl...
Embodiment 3
[0050] A new energy-saving brick and its processing technology. The weight ratio of the new energy-saving brick is: 300 parts of Portland cement, 710 parts of sand, 25 parts of expanded perlite, 30 parts of cinder, 15 parts of aluminum alloy, and 4 parts of straw , 7 parts of plant ash, 7 parts of thickening powder, 4 parts of deodorant additive, and 100 parts of clear water.
[0051] In the present invention, gallic tannic acid is used as the deodorizing aid, wherein the content of gallic tannic acid is 65%.
[0052] A new type of energy-saving brick processing technology, the production steps are as follows:
[0053] (1) Weigh and mix the raw materials. Firstly, Portland cement, sand, expanded perlite, cinder, aluminum alloy, straw, plant ash, thickened powder and clear water are evenly mixed according to weight parts, and evenly stirred. First, silicic acid Mix salt cement, sand, expanded perlite and cinder into clean water to make a mixture, then add aluminum alloy, straw...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com