Resin synthetic board and manufacturing method thereof
A technology of resin synthesis and production methods, applied in chemical instruments and methods, paper/cardboard layered products, lamination, etc., can solve problems such as non-wear resistance, easy peeling and falling, and uneven material quality. Achieve a smooth surface and not easy to peel
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] A resin composite board, which is pressed by a resin composite board and a decorative film covering the surface of the resin composite board, the resin composite board is made of the following components according to the mass percentage: 11% pine powder, 11% fir powder, Poplar wood powder 60%, zinc stearate 0.02%, titanium dioxide 0.02%, melamine formaldehyde resin 17.96%, the decorative film is made of solid paper impregnated with melamine formaldehyde resin.
[0027] A method for making a resin composite board, which is realized by the following steps:
[0028] (1) Drying: Dry the raw materials of pine wood powder, fir wood powder and poplar wood powder;
[0029] (2) Weighing: Accurately weigh 11% of dried pine wood powder, 11% of fir wood powder, 60% of poplar wood powder, 0.02% of zinc stearate, 0.02% of titanium dioxide, and 17.96% of melamine formaldehyde resin;
[0030] (3) Mixing and stirring: Send the above-mentioned pine wood powder, fir wood powder, poplar w...
Embodiment 2
[0034] A resin composite board, which is pressed by a resin composite board and a decorative film covering the surface of the resin composite board, the resin composite board is made of the following components according to the mass percentage: 14% pine powder, 14% fir powder, 40% poplar wood powder, 0.15% zinc stearate, 0.15% titanium dioxide, 31.7% melamine formaldehyde resin, and the decorative film is made of solid paper impregnated with melamine formaldehyde resin.
[0035] A method for making a resin composite board, which is realized by the following steps:
[0036] (1) Drying: Dry the raw materials of pine wood powder, fir wood powder and poplar wood powder;
[0037] (2) Weighing: Accurately weigh 14% of dried pine wood powder, 14% of fir wood powder, 40% of poplar wood powder, 0.15% of zinc stearate, 0.15% of titanium dioxide, and 31.7% of melamine formaldehyde resin;
[0038] (3) Mixing and stirring: Send the above-mentioned pine wood powder, fir wood powder, poplar...
Embodiment 3
[0042] A resin composite board, which is pressed by a resin composite board and a decorative film covering the surface of the resin composite board, the resin composite board is made of the following components according to the mass percentage: 13% pine powder, 13% fir powder, Poplar wood powder 50%, zinc stearate 0.1%, titanium dioxide 0.1%, melamine formaldehyde resin 23.8%, the decorative film is made of solid paper impregnated with melamine formaldehyde resin.
[0043] A method for making a resin composite board, which is realized by the following steps:
[0044] (1) Drying: Dry the raw materials of pine wood powder, fir wood powder and poplar wood powder;
[0045] (2) Weighing: Accurately weigh 13% of dried pine wood powder, 13% of fir wood powder, 50% of poplar wood powder, 0.1% of zinc stearate, 0.1% of titanium dioxide, and 23.8% of melamine formaldehyde resin;
[0046] (3) Mixing and stirring: Send the above-mentioned pine wood powder, fir wood powder, poplar wood po...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com