Preparation methods of Ti3O5 powder
A technology of powder and carbon black powder, applied in the direction of titanium oxide/hydroxide, etc., can solve the problems of unsafety, high cost, cumbersome operation, etc., and achieve high production efficiency and safety, low manufacturing cost, and simple process Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0045] In the present embodiment, adopt the first kind of preparation method described in the present invention to prepare Ti 3 o 5 Powder, the process steps are as follows:
[0046] (1) Ingredients
[0047] According to Ti 3 o 5 The chemical formula of the powder and the chemical reaction between the raw materials used are used to measure each raw material, and the weight percentage of each raw material is as follows:
[0048] Micron TiO 2 Powder 88.80wt%,
[0049] Micron titanium hydride powder 11.20wt%;
[0050] (2) Mixing and drying
[0051] Put the raw materials measured in step (1) into the roller ball mill, use WC-8wt%Co cemented carbide balls with a diameter of φ10mm as the grinding balls, the ball-to-material ratio is 8:1, and use 75% alcohol as the wet Grinding medium, the addition amount of which is limited to submerging the raw materials and grinding spheres, grinding and dispersing for 75 hours at a ball milling speed of 30 rpm to mix the raw materials evenl...
Embodiment 2
[0055] In the present embodiment, adopt the first kind of preparation method described in the present invention to prepare Ti 3 o 5 Powder, the process steps are as follows:
[0056] (1) Ingredients
[0057] According to Ti 3 o 5 The chemical formula of the powder and the chemical reaction between the raw materials used are used to measure each raw material, and the weight percentage of each raw material is as follows:
[0058] Nano-TiO 2 Powder 83.60wt%,
[0059] Nano titanium powder 16.40wt%;
[0060] (2) Mixing and drying
[0061] Put the measured raw materials in step (1) into the roller ball mill, use WC-8wt%Co cemented carbide balls with a diameter of φ10mm as the grinding balls, the ball-to-material ratio is 8:1, and use deionized water as the wet grinding medium , its addition is limited to submerging the raw materials and grinding spheres, grinding and dispersing for 70 hours at a ball milling speed of 40 revs / min, so that the raw materials are mixed evenly, a...
Embodiment 3
[0065] In the present embodiment, adopt the first kind of preparation method described in the present invention to prepare Ti 3 o 5 Powder, the process steps are as follows:
[0066] (1) Ingredients
[0067] According to Ti 3 o 5 The chemical formula of the powder and the chemical reaction between the raw materials used are used to measure each raw material, and the weight percentage of each raw material is as follows:
[0068] Micron TiO 2 Powder 92.42wt%,
[0069] Micron charcoal powder 7.58wt%;
[0070] (2) Mixing and drying
[0071] Put the raw materials measured in step (1) into the roller ball mill, use WC-8wt%Co cemented carbide balls with a diameter of φ10mm as the grinding balls, the ball-to-material ratio is 8:1, and use acetone as the wet grinding medium. The amount of addition is limited to submerge the raw materials and grinding spheres, grind and disperse for 80 hours at a ball milling speed of 30 rpm to mix the raw materials evenly, then sieve and separa...
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com