Environment-friendly ABS/PET (acrylonitrile-butadiene-styrene/polyethylene glycol terephthalate) alloy and preparation method thereof
An alloy and environmentally friendly technology, applied in the field of environmentally friendly ABS/PET alloy and its preparation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0053] A kind of environmental protection ABS / PET alloy, it is made up of the raw material of following weight part:
[0054] ABS 40 parts
[0055] 30 copies of recycled PET
[0056] Nano calcium carbonate 1 part
[0057] 3 parts heavy calcium carbonate
[0058] Acrylate and glycidyl ester difunctional vinyl elastomer 2 parts
[0059] Methyl methacrylate-butadiene-styrene terpolymer 3 parts
[0060] 0.2 parts of pentaerythritol stearate
[0061] Dilauryl thiodipropionate 0.2 parts.
[0062] Wherein, the butadiene content in the ABS is 28wt%, and the styrene content is 25wt%.
[0063] Wherein, the particle diameter of described nano-calcium carbonate is 160 nanometers.
[0064] Wherein, the particle diameter of described ground calcium carbonate is 2600 orders.
[0065] Wherein, the melt index of the acrylate and glycidyl ester bifunctional vinyl elastomer is 2.0 g / 10 min, and the grafting rate of the acrylate and glycidyl ester bifunctional vinyl elastomer is 3.0%.
...
Embodiment 2
[0074] A kind of environmental protection ABS / PET alloy, it is made up of the raw material of following weight part:
[0075] ABS 50 parts
[0076] 40 copies of recycled PET
[0077] Nano calcium carbonate 3 parts
[0078] 5 parts heavy calcium carbonate
[0079] Acrylate and glycidyl ester difunctional vinyl elastomer 4 parts
[0080] Methyl methacrylate-butadiene-styrene terpolymer 5 parts
[0081] 0.5 parts of pentaerythritol stearate
[0082] Dilauryl thiodipropionate 0.5 parts.
[0083] Wherein, the butadiene content in the ABS is 30wt%, and the styrene content is 30wt%.
[0084] Wherein, the particle diameter of described nano calcium carbonate is 200 nanometers.
[0085] Wherein, the particle diameter of described ground calcium carbonate is 3000 orders.
[0086] Wherein, the melt index of the acrylate and glycidyl ester difunctional vinyl elastomer is 3.0 g / 10 min, and the grafting rate of the acrylate and glycidyl ester bifunctional vinyl elastomer is 4.0%.
...
Embodiment 3
[0095] A kind of environmental protection ABS / PET alloy, it is made up of the raw material of following weight part:
[0096] ABS 60 parts
[0097] 45 copies of recycled PET
[0098] Nano calcium carbonate 4 parts
[0099] 4 parts heavy calcium carbonate
[0100] Acrylate and glycidyl ester difunctional vinyl elastomer 3 parts
[0101] Methyl methacrylate-butadiene-styrene terpolymer 6 parts
[0102] 0.2 parts of pentaerythritol stearate
[0103] Dilauryl thiodipropionate 1 part.
[0104] Wherein, the butadiene content in the ABS is 32wt%, and the styrene content is 29wt%.
[0105] Wherein, the particle diameter of described nano calcium carbonate is 220 nanometers.
[0106] Wherein, the particle diameter of described ground calcium carbonate is 3300 orders.
[0107] Wherein, the melt index of the acrylate and glycidyl ester bifunctional vinyl elastomer is 3 g / 10 min, and the grafting rate of the acrylate and glycidyl ester bifunctional vinyl elastomer is 5.0%.
[010...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
melt flow index | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com