Surface-sizing fixing agent for color ink-jet paper and preparation method and application thereof
A technology of surface sizing and color spray paper, applied in papermaking, textiles and papermaking, non-fiber pulp addition, etc., can solve the problems of low cationicity of styrene-acrylic emulsion, poor water resistance of color fixing agent, etc., and improve surface properties , solve the effect of poor hydrophobicity and increase cationic groups
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0033] The preparation method of color jet paper surface sizing color-fixing agent of the present invention comprises the following steps:
[0034] (1) Weigh 10 parts by mass of cationic starch CS-8, 0.04 parts by mass of ammonium persulfate, and 24 parts by mass of water into a water bath in a four-neck flask, start the stirrer, and gelatinize at 85°C for 1 hour;
[0035] (2) Add ferrous chloride solution prepared by 0.01 parts by mass of ferrous chloride and 1 part by mass of water into a four-necked flask;
[0036] (3) Add a hydrophilic monomer solution prepared by 3.5 parts by mass of maleic anhydride and 8.5 parts by mass of water into a four-necked flask;
[0037] (4) Add dropwise a hydrogen peroxide dilution diluted with 0.8 parts by mass of 30% hydrogen peroxide and 1.5 parts by mass of water into a four-necked flask;
[0038] (5) After mixing 20 parts of a mixture of styrene and butyl acrylate (the mass ratio of styrene and butyl acrylate is 5:4) and 5 parts of rosin...
Embodiment 2
[0043] The preparation method of color jet paper surface sizing color-fixing agent of the present invention comprises the following steps:
[0044] (1) Weigh 20 parts by mass of cationic starch CS-8, 0.08 parts by mass of ammonium persulfate, and 48 parts by mass of water into a water bath in a four-neck flask, start the stirrer, and gelatinize at 85°C for 1 hour;
[0045] (2) Add ferrous chloride solution prepared by 0.01 parts by mass of ferrous chloride and 2 parts by mass of water into a four-necked flask;
[0046] (3) Add a hydrophilic monomer solution prepared by 3.5 parts by mass of maleic anhydride and 17 parts by mass of water into a four-necked flask;
[0047] (4) Add dropwise a hydrogen peroxide dilution diluted with 0.8 parts by mass of 30% hydrogen peroxide and 3 parts by mass of water into a four-necked flask;
[0048] (5) Mix 35 parts by mass of styrene and butyl acrylate (the mass ratio of styrene and butyl acrylate is 5:4) and 5 parts by mass of rosin in a be...
Embodiment 3
[0053] The preparation method of color jet paper surface sizing color-fixing agent of the present invention comprises the following steps:
[0054] (1) Weigh 30 parts by mass of cationic starch CS-8, 0.12 parts by mass of ammonium persulfate, and 86.4 parts by mass of water into a water bath in a four-neck flask, start the stirrer, and gelatinize at 85°C for 1 hour;
[0055] (2) Add ferrous chloride solution prepared by 0.01 parts by mass of ferrous chloride and 3.6 parts by mass of water into a four-necked flask;
[0056] (3) Add a hydrophilic monomer solution prepared by 5.5 parts by mass of hydrophilic monomer (maleic anhydride to acrylamide mass ratio 1:1) and 30.6 parts by mass of water into a four-necked flask;
[0057] (4) Add dropwise the hydrogen peroxide dilution diluted with 0.8 parts by mass of 30% hydrogen peroxide and 54 parts by mass of water into the four-necked flask;
[0058] (5) Mix 25 parts by mass of styrene and butyl acrylate (the mass ratio of styrene a...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com