Looking for breakthrough ideas for innovation challenges? Try Patsnap Eureka!

Preparation method of dope for metal type casting of magnesium alloy thin-walled component

A metal mold casting, magnesium alloy technology, applied in casting molding equipment, metal processing equipment, coating and other directions, can solve the problem that cannot be applied to magnesium alloy, etc., and achieve the effect of reducing the amount of defects, good thermal insulation performance, and easy preservation

Active Publication Date: 2015-02-25
临泉县卡天下电子商务有限公司
View PDF9 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0005] It can be seen that the coatings used for metal molds of thin-walled parts in the prior art are all aimed at cast aluminum alloys, but there are few reports on magnesium alloys. Due to the difference in properties between magnesium alloys and aluminum alloys, it is impossible to use the coatings in the prior art. Metal mold casting coatings for thin-walled aluminum alloys are directly applied to magnesium alloys. Therefore, it is urgent to develop a metal mold casting coating suitable for magnesium alloy thin-walled parts

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0019] A method for preparing a coating for metal mold casting of magnesium alloy thin-walled parts. The coating is composed of the following components in terms of weight percentage: 1.5% of diatomite, 3% of magnesium oxide powder, 1.2% of titanium dioxide powder, and 2% of zircon powder %, bentonite 1.5%, asbestos powder 4%, silica sol 1.2%, and the balance is alcohol, and the described preparation method comprises the steps:

[0020] 1) Weigh the ingredients according to the above ratio;

[0021] 2) Take alcohol with 30% total weight of alcohol, add bentonite, stir to suspend, then add MgO powder, TiO 2 powder and zircon powder, stirred for 15 minutes, made it uniform, got the mixture I;

[0022] 3) Mix and stir diatomite, asbestos powder and silica sol for 20 minutes, add alcohol with a total weight of 20% alcohol, and stir for another 5 minutes to make it evenly mixed to obtain Mixture II;

[0023] 4) Mix the mixture I and the mixture II with the remaining 50% alcohol b...

Embodiment 2

[0025] A method for preparing a coating for metal mold casting of magnesium alloy thin-walled parts. The coating is composed of the following components in terms of weight percentage: 2.5% of diatomite, 2% of magnesium oxide powder, 1.8% of titanium dioxide powder, and 1% of zircon powder. %, bentonite 2.5%, asbestos powder 2%, silica sol 1.4%, and the balance is alcohol, and the described preparation method comprises the steps:

[0026] 1) Weigh the ingredients according to the above ratio;

[0027] 2) Take alcohol with 30% total weight of alcohol, add bentonite, stir to suspend, then add MgO powder, TiO 2 powder and zircon powder, stirred for 25 minutes, made it uniform, got the mixture I;

[0028] 3) Mix and stir diatomite, asbestos powder and silica sol for 10 minutes, add alcohol with a total weight of 20% alcohol, and stir for another 15 minutes to make it evenly mixed to obtain Mixture II;

[0029] 4) Mix the mixture I and the mixture II with the remaining 50% alcohol...

Embodiment 3

[0031] A method for preparing a coating for metal mold casting of magnesium alloy thin-walled parts. The coating is composed of the following components in terms of weight percentage: 2.0% of diatomite, 2.5% of magnesium oxide powder, 1.5% of titanium dioxide powder, and 1.5% of zircon powder %, bentonite 2.0%, asbestos powder 3.0%, silica sol 1.3%, and the balance is alcohol, and the described preparation method comprises the steps:

[0032] 1) Weigh the ingredients according to the above ratio;

[0033] 2) Take alcohol with 30% total weight of alcohol, add bentonite, stir to suspend, then add MgO powder, TiO 2 powder and zircon powder, stirred for 20 minutes, made it uniform, got the mixture I;

[0034] 3) Mix and stir diatomite, asbestos powder and silica sol for 15 minutes, add alcohol with a total weight of 20% alcohol, and stir for another 10 minutes to make it evenly mixed to obtain Mixture II;

[0035] 4) Mix the mixture I and the mixture II with the remaining 50% al...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses a preparation method of a dope for metal type casting of a magnesium alloy thin-walled component. The dope comprises the following components in percentage by weight: 1.5 to 2.5 percent of kieselguhr, 2 to 3 percent of magnesium oxide powder, 1.2 to 1.8 percent of titanium dioxide powder, 1 to 2 percent of zirconite powder, 1.5 to 2.5 percent of bentonite, 2 to 4 percent of asbestos powder, 1.2 to 1.4 percent of silica sol and the balance of alcohol. The preparation method comprises the following steps of 1) weighing the materials according to the proportion; 2) taking 30 percent of the total alcohol, adding the bentonite into the alcohol, stirring until the bentonite is suspended, sequentially adding the magnesium oxide powder, the titanium dioxide powder and the zirconite powder into the suspension, and stirring the suspension for about 15 to 25 minutes to uniformly mix the materials and obtain a mixture I; 3) mixing and stirring the kieselguhr, the asbestos powder and the silica sol for about 10 to 20 minutes, adding 20 percent of the total alcohol into the mixture, and stirring the materials for about 5 to 15 minutes to uniformly mix the materials and obtain a mixture II; and 4) mixing the mixture I, the mixture II and 50 percent of residual alcohol, and stirring the materials for about 20 to 30 minutes to obtain the dope.

Description

technical field [0001] The invention relates to the field of casting, in particular to a method for preparing a coating for metal mold casting of magnesium alloy thin-walled parts. Background technique [0002] Metal mold casting, also known as hard mold casting, is a casting method in which liquid metal is poured into metal molds to obtain castings. Cast molds are made of metal and can be used repeatedly (hundreds to thousands of times). The castings that metal mold casting can produce at present have certain restrictions in terms of weight and shape. For example, the weight of castings should not be too large; the wall thickness is also limited, and it is difficult to cast smaller castings with wall thickness. [0003] Due to the fast cooling rate of magnesium alloy thin-walled parts in the metal mold casting process, it is easy to form defects such as cold shut, pinholes and shrinkage porosity in the castings, so that the castings are scrapped. Therefore, how to improve ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): B22C3/00
Inventor 齐伟光李发旺
Owner 临泉县卡天下电子商务有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products