Method for manufacturing copper-tungsten contact
A production method and contact technology, which is applied in cable/conductor manufacturing, electrical components, circuits, etc., can solve the problems of insufficient copper phase, contact ablation, and low contact strength, so as to achieve sufficient and uniform fusion and improve performance Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] Follow these steps:
[0028] (1) Making tungsten billet: take 2100 parts of tungsten powder, 11 parts of forming agent, and 15 parts of wetting agent, mix and stir, and then put it into a molding mold for compression molding to obtain a tungsten billet;
[0029] (2) Making a graphite crucible: according to the size of the copper-tungsten contact to be made, select a corresponding graphite rod and process it to obtain a graphite crucible whose inner cavity is in the shape of a contact;
[0030] (3) Dry the graphite crucible: put the graphite crucible in an oven with a temperature of 500°C and keep it warm for more than 3 hours;
[0031] (4) Protect the graphite crucible: paint the graphite water agent or paste graphite paper on the inner wall of the graphite crucible, then put the graphite crucible into an oven with a temperature of 200°C and keep it warm for 3 hours;
[0032] (5) Prepare copper-containing materials: make copper materials according to the weight of the ...
Embodiment 2
[0038] (1) Making tungsten billet: take 2100 parts of tungsten powder, 11 parts of forming agent, and 15 parts of wetting agent, mix and stir, and then put it into a molding mold for compression molding to obtain a tungsten billet;
[0039] (2) Making a graphite crucible: according to the size of the copper-tungsten contact to be made, select a corresponding graphite rod and process it to obtain a graphite crucible whose inner cavity is in the shape of a contact;
[0040] (3) Dry the graphite crucible: put the graphite crucible in an oven with a temperature of 400°C and keep it warm for more than 5 hours;
[0041] (4) Protect the graphite crucible: paint graphite water or stick graphite paper on the inner wall of the graphite crucible, then put the graphite crucible into an oven with a temperature of 300°C and keep it warm for 1 hour;
[0042] (5) Prepare copper-containing materials: make chromium bronze according to the weight of the copper-tungsten contact to be made and the...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com