Method for producing single-sided composite stainless steel cold rolling base stock
A production method, stainless steel technology, applied in the direction of metal rolling, metal rolling, workpiece surface treatment equipment, etc., can solve the problems of low flatness of steel strip, difficulty in controlling hardness, insufficient shape and brightness of steel strip, etc., and achieve The effect of reducing unqualified products and reducing the defective rate
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0063] Embodiment 1: the specific implementation steps of the present invention are as follows:
[0064] 1. Substrate selection: carbon steel or low alloy steel
[0065] 1) The surface of the steel plate should be smooth and free of cracks, and defects in use, such as folds, cracks, scars, pitting, etc., are not allowed.
[0066] 2) The steel plate should be cut at right angles, and when the length dimension error is not less than 2 mm, the diagonal line between the length and width is not more than 5 mm.
[0067] 3) The incision must not have defects such as delamination and tearing.
[0068] 2. Surface treatment of substrate and double board:
[0069] Substrate: Grinding the surface oxide layer with a suspension wheel grinder
[0070] Grind the surface with a flap wheel until it is bright
[0071] Grinding surface depressions with an angle grinder
[0072] Doubler: Polish the surface to a bright finish with a fiber wheel
[0073] 3. Bl...
Embodiment 2
[0119] Embodiment 2: the specific implementation steps of the present invention are as follows:
[0120] 1. Substrate selection: carbon steel or low alloy steel
[0121] 1) The surface of the steel plate should be smooth and free of cracks, and defects in use, such as folds, cracks, scars, pitting, etc., are not allowed.
[0122] 2) The steel plate should be cut at right angles, and when the length dimension error is not less than 2 mm, the diagonal line between the length and width is not more than 5 mm.
[0123] 3) The incision must not have defects such as delamination and tearing.
[0124] 2. Surface treatment of substrate and double board:
[0125] Remove the surface oxide layer with a shot blasting machine.
[0126] If necessary, the substrate can be treated twice to achieve the purpose of removing the oxide layer.
[0127] 3. Blank assembly:
[0128] 3.1 Production of retaining strips:
[0129] 1) All the steel plates of the bar are carbon steel with a thickness o...
PUM
Property | Measurement | Unit |
---|---|---|
decomposition temperature | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com