Embodiment 1~6
[0016] Embodiment 1~6 prepares the hydroxyl acrylate emulsion containing phosphate group
[0017] (1) Raw materials and their proportioning (see Table 1).
[0018] Table 1
[0019] components
raw material name
Dosage
Example
1 Dosage
Example
2 Dosage
Example
3 Dosage
Example
4 Dosage
Example
5 Dosage
Example
6 Hydroxy-free Propylene
Ester monomer
Methyl methacrylate
Butyl acrylate
Isooctyl acrylate 100.0
127.5
80.0 120.0
100.0
105.0 70.0
150.5
99.5 120.0
89.0
106.0 130.0
97.5
70.0 110.0
117.5
100.0 Hydroxy-containing acrylic acid
Ester monomer Hydroxyethyl Acrylate
Hydroxypropyl Acrylate 70.0
/ /
60.0 60.0
/ 75.0
/ 80.0
/ 54.5
/ Phosphate-containing propane
acrylate monomer PAM-100
22.5
15.0
20.0
10.0
22.5
18.0
Initiator
Azobisisobutyronitrile
3.0
2.5
/
3.0
2.5
3.0
[0020]
Benzoyl p...
Embodiment 7
[0023] Example 7 Preparation of water-based two-component anti-corrosion coating
[0024] The defoamer TEGO815N, water-based dispersant TEGO715W, and thickener TEGO3000 used are all commercially available products from Germany Degussa Company.
[0025] (1) Preparation of pigment filler slurry
[0026] The components and dosage of the pigment filler paste are as follows:
[0027] iron red 30;
[0028] Zinc phosphate 12;
[0029] Mica powder 12;
[0030] Kaolin 16;
[0031] Deionized water 30;
[0032] Water-based dispersant (TEGO715W) 0.7;
[0033] After mixing the above components, use a sand mill to grind to a fineness of less than 50 microns, and store them for future use.
[0034] (2) Preparation of water-based two-component anti-corrosion coatings
[0035] Use the pigment filler slurry prepared above and the emulsion obtained in Example 1, mix them at a ratio of 1:1 by weight and add thickener TEGO3000 and defoamer TEGO815N, the addition amount of which is 1 / 2 of t...
Embodiment 8
[0038] Example 8 Preparation of water-based two-component anti-corrosion coating
[0039] (1) Preparation of pigment filler slurry
[0040] Identical to the formula and method of embodiment 7;
[0041] (2) Preparation of water-based two-component anti-corrosion coatings
[0042] Use the pigment filler slurry prepared above and the emulsion obtained in Example 2, mix them at a ratio of 1:1 by weight and add thickener TEGO3000 and defoamer TEGO815N, the addition amount of which is the total weight of the above mixture. 0.4% and 0.2%, mixed evenly is the first component;
[0043] Use the water-dispersed curing agent Bayhydur3100 produced by Bayer Company of Germany as the second component;
[0044] Mix component A and component B at a weight ratio of 6:1, and stir evenly to obtain the water-based two-component anti-corrosion coating of Example 8.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com