Embodiment example 1
[0048] Cu-BTC based composite phase change material
[0049] 1) Select a 500-mesh copper sieve with a volume of 2cm×2cm×1mm, immerse the copper sieve in acetone, methanol, and deionized water for 30 minutes, and dry them in a blast oven at 60°C each time to obtain the substrate for Cu-BTC growth ;
[0050] 2) Fully dissolve 7.021g of copper nitrate and 3.063g of trimesic acid in a mixed solution of 25mL of water and 25mL of ethanol, stir vigorously at room temperature for 30min to obtain a uniform solution, then move it into the reaction kettle, Put it in an oven and react at 95°C for 15 hours. After the reaction product is centrifuged and washed, put it in an oven and dry it at 80°C for 8 hours to obtain Cu-BTC. Dissolve the dried Cu-BTC in water to obtain Cu-BTC mother liquor, wherein The molar ratio of dried Cu-BTC powder to water is 1:25.
[0051] 3) Preheat the copper sieve in step 1) at 100°C for 10 minutes, at this temperature, drop the Cu-BTC mother liquor prepared i...
Embodiment example 2
[0055] Cr-MIL-101-NH 2 matrix composite phase change material
[0056] 1) Select a 500-mesh copper sieve with a volume of 2cm×2cm×1mm, immerse the copper sieve in acetone, methanol, and deionized water for 30 minutes, and then dry it in a blast oven at 60°C each time to obtain Cr-MIL-101- NH 2 growth base;
[0057] 2) Fully dissolve 3.2 g of 2-aminoterephthalic acid and 3.2 g of chromium nitrate nonahydrate in 60 mL of deionized water, add 0.8 g of sodium hydroxide and stir vigorously at room temperature for 30 min to obtain a uniform solution, then Move it into the reaction kettle, put it in an oven and react at 150°C for 12 hours, and after the reaction product is washed by centrifugation, put it in an oven and dry it at 80°C for 8 hours to obtain Cr-MIL-101-NH 2 , the dried Cr-MIL-101-NH 2 Dissolve in water to get Cr-MIL-101-NH 2 Mother liquor, wherein the dried Cr-MIL-101-NH 2 The molar ratio of powder and water is 1:25.
[0058] 3) Preheat the copper sieve in step ...
Embodiment example 3
[0061] MOF-5 based composite phase change materials
[0062] 1) Select a 500-mesh copper sieve with a volume of 2cm×2cm×1mm, immerse the copper sieve in acetone, methanol, and deionized water for 30 minutes, and dry them in a blast oven at 60°C each time to obtain the substrate for MOF-5 growth. ;
[0063] 2) Fully dissolve 0.69g of terephthalic acid and 3.41g of zinc nitrate hexahydrate in 100mL of DMF, stir vigorously at room temperature for 30min to obtain a uniform solution, then move it into a reaction kettle and put it in an oven for 100 ℃ for 18 hours, the reaction product was centrifuged and washed, put in an oven and dried at 80℃ for 8 hours to obtain MOF-5, and the dried MOF-5 was dissolved in water to obtain MOF-5 mother liquor, in which the dried MOF- 5 The molar ratio of powder and water is 1:25.
[0064] 3) Preheat the copper sieve treated in step 1) at 100°C for 10 minutes, at this temperature, drop the MOF-5 mother liquor prepared in step 2) onto the surface ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com