Flotation separation method of high grade lead-sulfur mixed concentrate
A technology of mixed concentrate and separation method, applied in flotation, solid separation, etc., can solve the problems of difficult dosing, poor process stability, high lead grade of sulfur concentrate, etc., to meet the requirements of industrial production and moderate foam stability , the effect of high metal recovery rate
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] In this embodiment, a high-lead, high-zinc, high-sulfur refractory ore in Yunnan is used as the raw material for implementation.
[0019] (1) Mineral raw materials
[0020] A refractory ore with high lead, high zinc and high sulfur in Yunnan, the raw ore lead grade is 5.67%, zinc grade is 17.52%, and iron grade is 14.84%. The ore mainly includes galena, sphalerite, pyrite, trace arsenopyrite, dolomite, calcite, followed by quartz and sericite.
[0021] (2) Pharmaceutical preparation and operating conditions
[0022] 1) Grind the high-grade lead-zinc-sulfur raw ore with a ball mill. The grinding fineness -0.074mm accounts for 65-70%. t, carry out lead-sulfur mixed flotation to obtain lead-sulfur mixed concentrate;
[0023] 2) Preparation of pyrite compound inhibitor:
[0024] a. Take 10 parts of sodium hydroxide and 0.1 part of fulvic acid to make a 40%wt solution, and stir at 70°C for 30 minutes; b. Take 6 parts of sodium sulfite and 4 parts of sodium thiosulfate to...
Embodiment 2
[0027] In this embodiment, a high-lead, high-zinc, high-sulfur refractory ore in Yunnan is used as the raw material for implementation.
[0028] (1) Mineral raw materials
[0029] A refractory ore with high lead, high zinc and high sulfur in Yunnan, the raw ore lead grade is 9.69%, zinc grade is 19.31%, and iron grade is 14.87%. The ore mainly includes galena, sphalerite, pyrite, dolomite, calcite, quartz and so on.
[0030] (2) Pharmaceutical preparation and operating conditions
[0031] 1) Grind the high-grade lead-zinc-sulfur raw ore with a ball mill. The grinding fineness -0.074mm accounts for 65-70%. t, carry out lead-sulfur mixed flotation to obtain lead-sulfur mixed concentrate;
[0032] 2) Preparation of pyrite compound inhibitor: same as Example 1.
[0033] 3) Add 1600g / t of the pyrite inhibitor, flotation after 20 minutes of pulping, and then add 600g / t of pyrite compound inhibitor, after one roughing, two beneficiation, two After the first sweep, the grade of l...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com