A high cleanliness, bamboo pulp technology, applied in pulp beating method, non-fiber pulp addition, fiber raw material processing and other directions, can solve the problems of easy transverse cutting, loss of pulp strength, and fiber hardening, etc., to improve softness. and strength, ensure the cleanliness of the paper surface, and the effect of good beating uniformity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0033] The pulping process of a kind of high-cleanliness primary color bamboo pulp of the present embodiment comprises the following steps:
[0034] Step a, transport the bamboo pulp to the pulp tower with softening liquid and fully soak and stretch for 24 hours, the amount of softening liquid is 20g / L to mix the pulp, then wash and dehydrate, separate the softening liquid, and obtain fully stretched pulp material;
[0035] The softening liquid is made by mixing the following raw materials in mass percentage:
[0038] Disodium edetate 0.15%
[0039] Sodium di-sec-octyl sulfonate maleate 1.2%
[0040] water balance.
[0041] Step b. The fully moistened pulp is first deslagged by a high-consistency slag remover, and then processed by a thickening device to make the concentration of the pulp reach 23%, and then transported to a high-consistency refiner for high-consistency beating, and at the same time, add a concentrat...
Embodiment 2
[0049] The pulping process of a kind of high-cleanliness primary color bamboo pulp of the present embodiment comprises the following steps:
[0050] Step a, transport the bamboo pulp to the pulp tower with softening liquid and fully soak and stretch for 28 hours. The amount of softening liquid is 16g / L to mix the pulp, then wash and dehydrate, separate the softening liquid, and obtain fully stretched pulp material;
[0051] The softening liquid is made by mixing the following raw materials in mass percentage:
[0052] Sodium peroxide 17%
[0053] Sodium sulfite 1%
[0054] Disodium edetate 0.1%
[0055] Sodium di-sec-octyl sulfonate maleate 1.5%
[0056] water balance.
[0057] Step b. The fully moistened pulp is firstly deslagged by a high-consistency slag remover, and then processed by a thickening device to make the concentration of the pulp reach 20%, and then transported to a high-consistency refiner for high-consistency beating, and at the same time, add a concentra...
Embodiment 3
[0065] The pulping process of a kind of high-cleanliness primary color bamboo pulp of the present embodiment comprises the following steps:
[0066] Step a, transport the bamboo pulp to the pulp tower with softening liquid and fully soak and stretch for 36 hours, the amount of softening liquid is 10g / L to mix the pulp, then wash and dehydrate, separate the softening liquid, and obtain fully stretched pulp material;
[0067] The softening liquid is made by mixing the following raw materials in mass percentage:
[0068] Sodium peroxide 18%
[0069] Sodium sulfite 3%
[0070] Disodium edetate 0.25%
[0071] Sodium di-sec-octyl sulfonate maleate 0.5%
[0072] water balance.
[0073] Step b. The fully moistened slurry is firstly deslagged by a high-consistency slag remover, and then processed by a thickening device to make the concentration of the slurry reach 25%, and then transported to a high-consistency refiner for high-consistency beating. At the same time, add a concentr...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com